Organosiloxy silicate ester with excellent emulsibility and preparation method thereof
The organic silanyloxy silicates were prepared by one-step method, and the reaction was carried out using acid solution, silicate solution and polyether coupling agent, which solved the problems of poor emulsification performance and environmental protection of the catalyst in the prior art, and achieved excellent emulsification of the product Effects and simplified process.
Patent Information
- Application Number
- CN202411074280.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the emulsification performance of organosilyloxy silicates is poor and the preparation process is complicated. The catalysts used, such as organotin substances, are limited by environmental protection requirements, and it is difficult to meet environmental protection needs.
The one-step method is used to prepare the organosilanoxy silicate with excellent emulsification. By mixing the acid solution, the silicate solution, the polyether coupling agent and the capping agent, the reaction is carried out and the solvent is neutralized to obtain the Product with excellent emulsification performance.
The emulsification performance of organosilyloxy silicates has been improved, the preparation process is simplified, the use of catalysts that are unfavorable to the environment is avoided, and the application value of the product is improved.
Smart Images

Figure CN118909257A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organosilicon alkoxy silicate synthesis, and specifically relates to an organosilicon alkoxy silicate with excellent emulsification and a preparation method thereof. Background Art
[0002] Silicone is a semi-inorganic, semi-organic structure. It has many excellent properties such as physiological inertness, lubricity, hydrophobicity, UV radiation resistance and compatibility, and is widely used in cosmetics, personal care, home furnishing, etc. Among them, silicone alkoxy silicate has a special structure, which is a double-layered compact spherical body. The core part is a cage-like SiO2 with a polymerization degree of 15 to 50, and the shell is R3SiO 0.5 When used, it often works synergistically with linear silicone oil to achieve the effects of viscosity increase, defoaming, and film formation.
[0003] Due to the improvement of environmental awareness in recent years, the demand for water-based materials has continued to increase. Due to its good hydrophobicity, organosilicon alkoxy silicate cannot be directly added to water-based materials. It is often added after emulsification to obtain its emulsion. Direct emulsification requires a large amount of emulsifiers, complex emulsification processes and equipment, and will introduce too much emulsifier into the addition system, which may have more negative effects. In order to improve the emulsification performance of organosilicon alkoxy silicate, it is often achieved by introducing polyether segments into organosilicon alkoxy silicate.
[0004] The prior art patent CN109810261A discloses a polyether-containing organosilicon alkoxysilicate, which is prepared by an addition reaction between a methyl hydrogen-containing resin and a terminal hydroxyl allyl polyether. The method requires first obtaining a methyl hydrogen-containing resin, and then, after a high-temperature addition reaction for several hours, further reacting the resin with anhydride, alkaline water, and the like at high temperatures. The whole process is complicated and time-consuming, and is further limited by the raw material stability of the methyl hydrogen-containing silicone resin.
[0005] In the prior art, the polyether-containing organosilicon alkoxy silicate described in the patent with publication number CN115926523A is obtained by mixing, heating and condensing a polyether compound and a Si-OH-containing organosilicon alkoxy silicate as raw materials under the condition of an organotin catalyst. The process is complicated and the catalyst used is mostly organotin, which is a restricted substance in the increasingly stringent environmental protection requirements of multiple industries.
[0006] Therefore, based on this, the technical solution of the present invention is proposed. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides an organosilicon alkoxy silicate with excellent emulsification performance, which contains a polyether group and is prepared by a one-step method, and the preparation method is simple.
[0008] The scheme of the present invention is to provide an organosilicon alkoxy silicate with excellent emulsification, which is prepared from the following raw materials: component A, component B, component C and component D; wherein:
[0009] The component A is an acidic solution;
[0010] The component B is a silicate solution;
[0011] The C component is a polyether coupling agent and a phase transfer agent;
[0012] The D component is a capping agent.
[0013] Preferably, the acidic solution is a hydrochloric acid solution or a sulfuric acid solution;
[0014] and / or, the silicate is potassium silicate or sodium silicate, and the modulus is 2.8 to 3.2;
[0015] And / or, the phase transfer agent is ethanol or isopropanol.
[0016] Preferably, the polyether coupling agent is (XO) a SiMe 3-a R 1 ;
[0017] And / or, the capping agent is Me3SiOSiMe3;
[0018] in:
[0019] X is methyl or ethyl, Me is methyl;
[0020] a is 2 or 3;
[0021] R 1 The structure is of formula (I) or formula (II);
[0022]
[0023] m, n are natural numbers, m<15, n<15;
[0024] R 2 It is -CH2CH=CH2 or -CH3.
[0025] Preferably, the preparation method of the polyether coupling agent is:
[0026] The aminosilane coupling agent, epoxy polyether and solvent are mixed, and heated to react under stirring conditions, and the polyether coupling agent is obtained after completion.
[0027] Preferably, the aminosilane coupling agent is (XO) a SiMe 3-a (CH2)3NH(CH2)2NH2 or (XO)a SiMe 3-a (CH2)3NH2;
[0028] And / or, the epoxy polyether is CH2OCHCH2(OC2H4) m (OC3H6) n OR 2 ;
[0029] And / or, the solvent is ethanol or isopropanol;
[0030] in:
[0031] X is methyl or ethyl, Me is methyl;
[0032] a is 2 or 3;
[0033] m, n are natural numbers, m<15, n<15;
[0034] R 2 It is -CH2CH=CH2 or -CH3.
[0035] Preferably, the temperature of the heating reaction is 50-80°C, and the heating reaction time is 5-8h;
[0036] And / or, the molecular weight of the epoxy polyether is 300-1000;
[0037] And / or, the molar ratio of the NH bonds in the epoxy polyether and the aminosilane coupling agent is 1.0-1.3:1.
[0038] Based on the same technical concept, another embodiment of the present invention is to provide a method for preparing an organosilicon alkoxysilicate having excellent emulsification properties, the preparation method comprising the following steps:
[0039] (1) mixing component A and component B, reacting under stirring conditions to obtain polysilicic acid;
[0040] (2) After the components A and B react for 20-600 seconds, the component C is added, and after the component C is added for 10-300 seconds, the component D is added to obtain a reaction solution after the reaction;
[0041] (3) allowing the reaction solution to stand for stratification to obtain an upper layer solution; and sequentially neutralizing and removing the solvent from the upper layer solution to obtain the organosilicon alkoxy silicate having excellent emulsification properties.
[0042] Preferably, the mass of the polyether coupling agent in the component C is 20-50% of the mass of SiO2 in the silicate in the component B.
[0043] The beneficial effects of the present invention are:
[0044] The present invention selects a difunctional or trifunctional polyether silane coupling agent, and first reacts it with a capping agent and a silicate, and then caps the silicate after the polyether chain segment is fully reacted into the resin structure; the polyether silane coupling agent selected by the present invention is prepared by reacting a commercially available amino-containing coupling agent with an epoxy-containing polyether, and does not require post-treatment after the reaction, and is directly added to the next step of synthesis, and the entire preparation process is simple; the polyether grafted silicone alkoxy silicate finally prepared has excellent emulsifying properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0046] Figure 1 This is the appearance picture of the lotion.
[0047] Figure 2 This is the particle size distribution diagram of Example 1 after emulsification.
[0048] Figure 3 This is the particle size distribution diagram of Example 2 after emulsification.
[0049] Figure 4 This is the particle size distribution diagram of Example 3 after emulsification.
[0050] Figure 5 This is the particle size distribution diagram of Example 4 after emulsification. DETAILED DESCRIPTION
[0051] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0052] Example 1
[0053] This embodiment provides a method for preparing an organosilicon alkoxy silicate with excellent emulsification properties, the preparation method comprising:
[0054] (I) Preparation of polyether coupling agent
[0055] In a reactor equipped with a thermostat, a temperature detector and a stirring device, 19.13 g of an amino coupling agent (CH3CH2O)2SiMe(CH2)3NH2, 75.6 g of epoxy polyether CH2OCHCH2(OC2H4)6OCH2CH=CH2, and 94.73 g of isopropanol were added in sequence, the stirring speed was set to 500 r / min, the internal temperature was maintained at 70°C and the reaction was carried out for 6 hours to prepare a polyether coupling agent solution;
[0056] (II) Preparation of organosilicon alkoxysilicate with excellent emulsification properties
[0057] (1) Add 100 g of 30% hydrochloric acid solution of component A to a reactor equipped with a thermostat, a temperature measuring device and a stirring device, set the stirring speed to 300 r / min, set the thermostat to 25° C., and add 250 g of 20% sodium silicate solution (modulus 3.2) of component B at one time under stirring, and obtain polysilicic acid after reaction;
[0058] (2) After the addition of component B is completed, add component C to the reactor for 70 seconds: 36 g of the polyether coupling agent solution prepared in step (I) and 140 g of isopropanol;
[0059] (3) After 3 minutes, 150 g of hexamethyldisiloxane was added at once, and the temperature was raised to 50°C for 2 hours. The mixture was allowed to stand for stratification, and the upper layer was a solution containing the target product.
[0060] (4) The upper layer is neutralized with aqueous ammonia and the solvent is removed by distillation to obtain an organosilicon alkoxysilicate having excellent emulsification properties.
[0061] Example 2
[0062] This embodiment provides a method for preparing an organosilicon alkoxy silicate with excellent emulsification properties, the preparation method comprising:
[0063] (I) Preparation of polyether coupling agent
[0064] In a reactor equipped with a thermostat, a temperature meter and a stirring device, 20.64 g of an amino coupling agent (CH3O)2SiMe(CH2)3NH(CH2)2NH2, 125.8 g of epoxy polyether CH2OCHCH2(OC2H4)4(OC3H6)2OCH2CH=CH2, and 146.5 g of isopropanol were added in sequence, the stirring speed was set to 500 r / min, the internal temperature was maintained at 70°C and the reaction was carried out for 8 hours to prepare a polyether coupling agent solution;
[0065] (II) Preparation of organosilicon alkoxysilicate with excellent emulsification properties
[0066] (1) Add 100 g of 15% sulfuric acid solution of component A to a reactor equipped with a thermostat, a temperature measuring device and a stirring device, set the stirring speed to 300 r / min, set the thermostat to 25° C., and add 300 g of 15% sodium silicate solution (modulus 3.2) of component B at one time under stirring, and obtain polysilicic acid after reaction;
[0067] (2) After the addition of component B is completed, count for 100 seconds and add component C: 30 g of the polyether coupling agent solution prepared in step (I) and 130 g of isopropanol to the reactor;
[0068] (3) After 5 minutes, 150 g of hexamethyldisiloxane was added at once, and the temperature was raised to 45°C for 3 hours. The mixture was allowed to stand for stratification, and the upper layer was a solution containing the target product.
[0069] (4) The upper layer is neutralized with aqueous ammonia and the solvent is removed by distillation to obtain an organosilicon alkoxysilicate having excellent emulsification properties.
[0070] Example 3
[0071] This embodiment provides a method for preparing an organosilicon alkoxy silicate with excellent emulsification properties, the preparation method comprising:
[0072] (I) Preparation of polyether coupling agent
[0073] In a reactor equipped with a thermostat, a temperature detector and a stirring device, 17.9 g of an amino coupling agent (CH3O)2SiMe(CH2)3NH2, 89.3 g of epoxy polyether CH2OCHCH2(OC2H4)4(OC3H6)2OCH2CH=CH2, and 100.7 g of isopropanol were added in sequence, the stirring speed was set to 800 r / min, the internal temperature was maintained at 70°C and the reaction was carried out for 6 hours to prepare a polyether coupling agent solution;
[0074] (II) Preparation of organosilicon alkoxysilicate with excellent emulsification properties
[0075] (1) Add 120 g of 30% hydrochloric acid solution of component A to a reactor equipped with a thermostat, a temperature measuring device and a stirring device, set the stirring speed to 300 r / min, set the thermostat to 20° C., and add 250 g of 18% potassium silicate solution (modulus 2.8) of component B at one time under stirring, and obtain polysilicic acid after reaction;
[0076] (2) After the addition of component B is completed, add component C to the reactor: 30 g of the polyether coupling agent solution prepared in step (I) and 200 g of ethanol;
[0077] (3) After 3 minutes, 180 g of hexamethyldisiloxane was added at once, and the temperature was raised to 50°C for 2 hours. The mixture was allowed to stand for stratification, and the upper layer was a solution containing the target product.
[0078] (4) The upper layer is neutralized with aqueous ammonia and the solvent is removed by distillation to obtain an organosilicon alkoxysilicate having excellent emulsification properties.
[0079] Example 4
[0080] This embodiment provides a method for preparing an organosilicon alkoxy silicate with excellent emulsification properties, the preparation method comprising:
[0081] (I) Preparation of polyether coupling agent
[0082] In a reactor equipped with a thermostat, a temperature detector and a stirring device, 17.9 g of an amino coupling agent (CH3O)2SiMe(CH2)3NH2, 95.9 g of epoxy polyether CH2OCHCH2(OC2H4)6(OC3H6)OCH2CH=CH2, and 111.8 g of isopropanol were added in sequence, the stirring speed was set to 800 r / min, the internal temperature was maintained at 70°C and the reaction was carried out for 6 hours to prepare a polyether coupling agent solution;
[0083] (II) Preparation of organosilicon alkoxysilicate with excellent emulsification properties
[0084] (1) Add 150 g of 15% sulfuric acid solution of component A to a reactor equipped with a thermostat, a temperature detector and a stirring device, set the stirring speed to 300 r / min, set the thermostat to 15° C., and add 280 g of 20% potassium silicate solution (modulus 2.8) of component B at one time under stirring, and obtain polysilicic acid after reaction;
[0085] (2) After the addition of component B is completed, add component C to the reactor for 80 seconds: 38 g of the polyether coupling agent solution prepared in step (I) and 180 g of isopropanol;
[0086] (3) After 4 minutes, 180 g of hexamethyldisiloxane was added at once, and the temperature was raised to 50°C for 2 hours. The mixture was allowed to stand for stratification, and the upper layer was a solution containing the target product.
[0087] (4) The upper layer is neutralized with aqueous ammonia and the solvent is removed by distillation to obtain an organosilicon alkoxysilicate having excellent emulsification properties.
[0088] Verification Example
[0089] The organosilicon alkoxy silicate obtained in Examples 1 to 4 was emulsified using the following process:
[0090] S1. In a reactor having a thermostat, a temperature detector and a stirring device, 50 g of organosilicon alkoxy silicate and 10 g of isomeric tridecanol polyoxyethylene polyether (TO-5) were added successively at a speed of 50 rpm and the internal temperature was maintained at 60 ° C and mixed for 2 h;
[0091] S2. The internal temperature was brought to 50°C, 40 g of deionized water at 50°C was added, the speed was maintained at 100 rpm, and the internal temperature was maintained at 50°C for 0.5 h;
[0092] S3. Increase the speed to 500 rpm, maintain the internal temperature at 50°C and mix for 3 hours;
[0093] S4. Add 100 g of deionized water at a temperature of 50° C., maintain the internal temperature at 50° C. and mix for 2 h, stop stirring, cool down, and obtain an emulsion of organosilicon alkoxy silicate.
[0094] The appearance of the emulsion of the organosilicon alkoxy silicate emulsified in the above four embodiments is as follows: Figure 1 The particle size test data are shown in Table 1. The results show that the organosilicon alkoxy silicates obtained in Examples 1 to 4 all have excellent emulsifying effects.
[0095] The particle size distribution diagrams of Examples 1 to 4 are as follows: Figure 2 to Figure 5 shown.
[0096] Table 1
[0097] Group Particle size / nm PDI Example 1 53.98 0.074 Example 2 39.71 0.053 Example 3 59.73 0.15 Example 4 45.72 0.082
[0098] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. An organosilicon alkoxysilicate having excellent emulsification properties, characterized in that: Prepared from the following raw materials: component A, component B, component C and component D; wherein: The component A is an acidic solution; the acidic solution is a hydrochloric acid solution or a sulfuric acid solution; The B component is a silicate solution; the silicate is potassium silicate or sodium silicate, and the modulus is 2.8 to 3.2; The C component is a polyether coupling agent and a phase transfer agent; the phase transfer agent is ethanol or isopropanol; The D component is a capping agent.
2. The organosilicon alkoxysilicate having excellent emulsification properties according to claim 1, characterized in that: The polyether coupling agent is (XO) a SiMe 3-a R 1 ; And / or, the capping agent is Me3SiOSiMe3; in: X is methyl or ethyl, Me is methyl; a is 2 or 3; R 1 The structure is of formula (I) or formula (II); m, n are natural numbers, m<15, n<15; R 2 It is -CH2CH=CH2 or -CH3.
3. The organosilicon alkoxysilicate having excellent emulsification properties according to claim 1, characterized in that: The preparation method of the polyether coupling agent is: The aminosilane coupling agent, epoxy polyether and solvent are mixed, heated to 50-80° C. under stirring conditions and reacted for 5-8 hours, and the polyether coupling agent is obtained after completion.
4. The organosilicon alkoxysilicate having excellent emulsification properties according to claim 3, characterized in that: The aminosilane coupling agent is (XO) a SiMe 3-a (CH2)3NH(CH2)2NH2 or (XO) a SiMe 3-a (CH2)3NH2; And / or, the epoxy polyether is CH2OCHCH2(OC2H4) m (OC3H6) n OR 2 ; And / or, the solvent is ethanol or isopropanol; in: X is methyl or ethyl, Me is methyl; a is 2 or 3; m, n are natural numbers, m<15, n<15; R 2 It is -CH2CH=CH2 or -CH3.
5. The organosilicon alkoxysilicate having excellent emulsification properties according to claim 3, characterized in that: The molecular weight of the epoxy polyether is 300-1000; And / or, the molar ratio of the epoxy polyether to the H directly connected to the N in the aminosilane coupling agent is 1.0-1.3:
1.
6. The method for preparing the organosilicon alkoxysilicate having excellent emulsification properties according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) mixing component A and component B, reacting under stirring conditions to obtain polysilicic acid; (2) After the components A and B react for 20-600 seconds, the component C is added, and after the component C is added for 10-300 seconds, the component D is added to obtain a reaction solution after the reaction; (3) allowing the reaction solution to stand for stratification to obtain an upper layer solution; and sequentially neutralizing and removing the solvent from the upper layer solution to obtain the organosilicon alkoxy silicate having excellent emulsification properties.
7. The method for preparing the organosilicon alkoxysilicate with excellent emulsification according to claim 6, characterized in that: The mass of the polyether coupling agent in the C component is 20-50% of the mass of SiO2 in the B component silicate.