Fireproof PP recycled material for new energy and preparation method thereof

By using light flame retardants such as expanded perlite powder and maleic anhydride compatible agents in PP recycling materials, their flame retardant performance is enhanced, and the mechanical and flame retardant performance of components such as new energy vehicle interior parts is solved. The problem has achieved light quality, energy conservation and safety improvement.

CN118909351APending Publication Date: 2024-11-08DONGGUAN YUJIE IND INVESTMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093153.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing PP recycled materials have insufficient mechanical properties and flame retardant performance in new energy vehicle interior parts, charging bag shells, and energy storage battery shells, resulting in increased weight, increased energy consumption, and risk of combustion and damage.

Method used

Use expanded perlite powder, porous silica aerogel, microporous calcium silicate, and zeolite powder as light flame retardant, combined with maleic anhydride compatible agent to prepare flame retardant compatible agents for recycling with PP The mixture of materials enhances its flame retardant, heat retardant, insulation and toughening properties.

Benefits of technology

It improves the flame retardant performance, toughness and insulation of fireproof PP recycling recycled materials, reduces the risks of combustion and damage, achieves the effect of light mass and energy saving, and meets the "light mass" requirements of new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987138440000051
    Figure BDA0004987138440000051
  • Figure BDA0004987138440000061
    Figure BDA0004987138440000061
  • Figure BDA0004987138440000101
    Figure BDA0004987138440000101
Patent Text Reader

Abstract

The invention relates to a fireproof PP recycled material for new energy and a preparation method thereof. The PP reclaimed material is prepared from the following raw materials in parts by weight: a PP reclaimed material, a plasticizer, a flame retardant, a lubricant and an anti-aging agent, the flame-retardant material is composed of a light flame retardant and a flame-retardant compatilizer; the light flame retardant is composed of one or more of expanded perlite powder, porous silicon dioxide aerogel, microporous calcium silicate and zeolite powder. Expanded perlite powder, porous silicon dioxide aerogel, microporous calcium silicate and zeolite powder are used as light flame retardants, a flame-retardant compatilizer is combined, a flame-retardant material is obtained and fully and uniformly mixed with a PP recycled material, and under the auxiliary action of a plasticizer, the flame-retardant material, a lubricating agent and an anti-aging agent, the flame-retardant material and the PP recycled material are fully and uniformly mixed; the obtained fireproof PP recycled material has the advantages of better flame retardant property, impact toughness and heat resistance, reduction of the possibility of combustion, damage and the like, light weight, reduction of source loss and better energy-saving effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polymer material processing, and more specifically, to a fireproof PP recycled material for new energy and a preparation method thereof. Background Art

[0002] With the advancement of science and technology, all walks of life focus on environmental protection and energy conservation, especially in the use of raw materials and energy. At present, the rapid development of new energy vehicles has gradually replaced traditional gasoline-burning vehicles, reducing the environmental pollution caused by gasoline combustion.

[0003] New energy vehicles are designed with "environmental protection" and "lightweight" as their main design concepts. Traditional automotive interior parts and assembly parts mostly use metal shells, which also makes them heavy, so the driving process consumes a lot of energy, which is not conducive to the effective use of resources.

[0004] Currently, automotive interior parts, automotive charging pack shells, and automotive energy storage battery shells all use thermoplastic resins with flame retardant effects to reduce the weight of the car and better play an energy-saving role. Commonly used resins include ABS, PET, PA, PP, etc. Among them, PP is widely used because of its better anti-flame retardant effect, light weight, and low price.

[0005] However, PP is obtained by extracting raw materials from petroleum and then processing them. This process will produce a large amount of carbon dioxide and consume energy. In order to save resources, PP waste is recycled again, but the mechanical properties and flame retardant properties of PP waste are low. Glass fiber, silica, boron nitride, flame retardant ABS, antimony trioxide, etc. are usually added to enhance its performance.

[0006] Although the addition of the above materials improves the mechanical properties and flame retardant properties of PP recycled materials to a certain extent, it also leads to an increase in the mass of PP recycled materials, and the weight of the produced automotive interior parts, the casing of the car's charging pack, and the casing of the car's energy storage battery increases, resulting in an increase in the energy consumption of the car, which is not conducive to energy saving; at the same time, breakage and burning will still occur during use, so further research is needed. Summary of the invention

[0007] In order to obtain lighter weight and better toughness and fire resistance, the present application provides a fire-resistant PP recycled material for new energy and a preparation method thereof.

[0008] In the first aspect, the present application provides a fire-resistant PP recycled material for new energy, comprising the following raw material components in parts by weight: PP recycled material 100 pieces Plasticizer 2-8 parts Flame retardant 30-80 parts Lubricant 1-5 parts 1-2 parts of anti-aging agent; The flame retardant material is composed of a light flame retardant and a flame retardant compatibilizer in a weight ratio of 10:(3.7-5.5); The lightweight flame retardant is one or more of expanded pearlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder.

[0009] Expanded perlite powder, porous silica aerogel, microporous calcium silicate, and zeolite powder all have low thermal conductivity, insulation, filling and toughening effects, and have the advantage of light weight compared to silica, boron nitride, etc. Therefore, this application uses a lightweight flame retardant composed of one or more of expanded perlite powder, porous silica aerogel, microporous calcium silicate, and zeolite powder, and then cooperates with the flame retardant compatibilizer of this application to play a better toughening, flame retardant, heat resistance and insulation role, reducing the possibility of burning or damage of fireproof PP recycled materials. The flame retardant compatibilizer can be selected from maleic anhydride grafted PP, etc.

[0010] The PP recycled material of the present application is obtained by recycling PP lunch boxes, PP washing machine shells, PP washing machine turbine shells, etc., and then undergoing a recycling process such as cleaning, impurity removal, and oil removal. It has the advantages of environmental protection, energy saving, and effective utilization of resources.

[0011] In summary, by using one or more of expanded perlite powder, porous silica aerogel, microporous calcium silicate, and zeolite powder as lightweight flame retardants, combined with flame retardant compatibilizers, the flame retardant material is fully and evenly mixed with the PP recycled material, and with the auxiliary action of plasticizers, flame retardants, lubricants, and anti-aging agents, the obtained fireproof PP recycled material has better flame retardant properties, toughness, insulation and heat resistance. When the new energy products produced are used, the possibility of combustion and breakage is reduced, and its durability and safety of use are improved. In addition, it is light in weight, reduces the energy loss of automobiles, and plays a better energy-saving role.

[0012] Heat resistance is the ability to reduce heat transfer, thereby reducing the chance of material burning. The lower the thermal conductivity, the more heat transfer can be prevented, thus achieving better flame retardant and heat resistance effects.

[0013] Preferably, the weight ratio of the expanded pearlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder is (2-3.2):(4-4.8):1:(1-2).

[0014] When expanded perlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder are compounded, they play a better synergistic role, and with the flame retardant compatibilizer, the obtained fireproof PP recycled materials play a better role in flame retardancy, heat resistance, insulation and toughening, reducing the possibility of burning, electric shock and breakage of new energy accessories, improving their safety and environmental protection. And light weight, reduce energy consumption and save resources.

[0015] Preferably, the particle size of the porous silica aerogel is 100-300 nm; the particle sizes of the expanded pearlite powder, microporous calcium silicate and zeolite powder are all 2-8 μm.

[0016] The above particle size range is the best choice for this application, and the particle size in this range is used for fire-proof PP recycled materials. When combined with flame retardant compatibilizers, the obtained fire-proof PP recycled materials have fire-proof, toughening, heat-resistant, and insulating effects.

[0017] Preferably, the flame retardant compatibilizer is prepared from the following raw materials in parts by weight: Phosphate acrylate monomer 1-3 parts Tris(2-hydroxyethyl)isocyanuric acid triacrylate 0.08-0.35 parts 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsilyloxy)disiloxane 0.1-0.5 parts Maleic anhydride compatibilizer 2-5 parts Initiator 0.01-0.03 parts 3-8 parts of diluent.

[0018] Phosphate acrylate monomers, tris(2-hydroxyethyl)isocyanurate triacrylate, and 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane contain phosphate groups, N groups, and siloxy groups, respectively, and thus all play a flame retardant role. In addition, when combined with anhydride compatibilizers, they play a better role in promoting compatibility with lightweight flame retardants, so that the flame retardant material prepared has better flame retardancy, heat resistance, compatibility, insulation, and toughness enhancement, and has the advantage of being light in weight.

[0019] When flame retardant fuel is used in the production of fireproof PP recycled materials, it can further improve the toughness, flame retardancy, insulation, etc. of the fireproof PP recycled materials and make them lighter. When used in the production of various accessories or auxiliary parts for new energy vehicles, it can play a better efficiency-enhancing role, thereby reducing the possibility of breakage and burning, while reducing energy loss.

[0020] Furthermore, the flame retardant compatibilizer is prepared by the following method: Weigh a phosphate acrylate monomer and an initiator, mix them evenly, heat to 60-70°C, react for 1-2h, add 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, mix evenly, react for 10-30min, then add tris(2-hydroxyethyl)isocyanuric acid triacrylate, mix evenly, react for 20-30min, then add a maleic anhydride compatibilizer and a diluent, mix evenly, neutralize, perform reduced pressure distillation, and solidify to obtain a flame retardant compatibilizer.

[0021] Preferably, the phosphate ester acrylate monomer is one or more of 2-hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate.

[0022] 2-Hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate contain phosphate groups, and the formed polymers have a certain flame retardant effect. They are combined with tri(2-hydroxyethyl)isocyanuric acid triacrylate and 1,3-bis(3-methacryloyloxypropyl)tetrakis(trimethylsiloxy)disiloxane to make the cross-linked polymer have better flame retardant effect and compatibility. They are then compounded with maleic anhydride compatibilizers to obtain flame retardant compatibilizers with better flame retardant effect, compatibility and toughening effect. Therefore, they can improve the compatibility of lightweight flame retardants and play a role in toughening, heat resistance, insulation and flame retardancy for fire-resistant PP recycled materials.

[0023] Preferably, the weight ratio of the 2-hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate is (1-7.5):(1-2.5):1.

[0024] When 2-hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate are compounded in the above-mentioned dosage, a better synergistic effect is achieved, and a flame retardant compatibilizer is obtained by combining tri(2-hydroxyethyl)isocyanurate triacrylate, 1,3-bis(3-methacryloyloxypropyl)tetrakis(trimethylsiloxy)disiloxane, and maleic anhydride compatibilizers, which interact with the lightweight flame retardant to further improve the toughness, insulation, heat resistance, and flame retardancy of the fire-resistant PP recycled materials.

[0025] Preferably, the maleic anhydride compatibilizer is one or more of maleic acid resin, maleic anhydride grafted PP, and maleic anhydride grafted SEBS.

[0026] Maleic acid resin, maleic anhydride grafted PP, and maleic anhydride grafted SEBS all have the function of improving the compatibility of lightweight flame retardants with PP recycled materials. In addition, the flame retardant compatibilizer prepared by combining with a cross-linked polymer made from phosphate acrylate monomers, tris(2-hydroxyethyl)isocyanuric acid triacrylate, and 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane can further improve the compatibility of lightweight flame retardants with PP recycled materials, and has a better toughening and flame retardant effect on PP recycled materials, further improving the insulation, flame retardancy, heat resistance, and toughness of fire-resistant PP recycled materials, and reducing the possibility of combustion and breakage.

[0027] Preferably, the weight ratio of the maleic acid resin, maleic anhydride grafted PP, and maleic anhydride grafted SEBS is (0.5-1):2:(0.8-1.3).

[0028] When maleic acid resin, maleic anhydride grafted PP, and maleic anhydride grafted SEBS are used, a synergistic toughening effect is achieved, and the insulation, flame retardancy, and toughness of the fire-resistant PP recycled materials are better.

[0029] Preferably, the antioxidant is one or more of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, antioxidant 168, UV770, UV-P, UV531, and UV-327; The lubricant is one or more of PETS, EBS, PE wax and triphenyl phosphate; The plasticizer is one or more of glyceryl tribenzoate, acetyl tributyl citrate, 1,2-cyclohexanedicarboxylic acid diisopropyl ester, and acetylated cyclohexanol acetyl ricinoleate.

[0030] The use of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, and antioxidant 168 has a better antioxidant effect, further improving the anti-aging properties of fireproof PP recycled materials; while UV770, UV-P, UV531, and UV-327 have a better anti-ultraviolet aging effect, and can also further improve the anti-aging properties.

[0031] One or more of PETS, EBS, PE wax and triphenyl phosphate are used as lubricants to assist in the processing of fire-resistant PP recycled materials and improve processing convenience.

[0032] Glyceryl tribenzoate, acetyl tributyl citrate, diisopropyl 1,2-cyclohexanedicarboxylate, and acetylated cyclohexanol acetylic ricinoleate are used as plasticizers to play a plasticizing role, and are compounded with flame retardant fuels to make the insulation, flame retardancy and toughness of the fire-resistant PP recycled materials better.

[0033] In the second aspect, the present application provides a method for preparing fireproof PP recycled materials for new energy, which is prepared by the following method: Weigh the flame retardant compatibilizer and heat it until it is melted, then add the light flame retardant and mix evenly, cool, crush, and sieve to obtain the flame retardant; weigh the recycled material, plasticizer, flame retardant, lubricant, and anti-aging agent according to weight parts, mix evenly, extrude, cool, and granulate to obtain the fireproof PP recycled material.

[0034] In the above process, the operation is simple and the production efficiency is high. The flame retardant compatibilizer is heated to melt, and then the light flame retardant is added to make it fully mixed and coated. After cooling, the formed solid is crushed to obtain a flame retardant material, which is easy to mix evenly with recycled materials, plasticizers, lubricants, and anti-aging agents. After the extrusion process, the materials are fully mixed, so that the obtained fire-resistant PP recycled materials have better insulation, flame retardancy and toughness.

[0035] In summary, this application has the following beneficial effects: 1. By using one or more of expanded perlite powder, porous silica aerogel, microporous calcium silicate, and zeolite powder as lightweight flame retardants, combined with flame retardant compatibilizers, flame retardant fuel is obtained, which is fully mixed with PP recycled materials, and with the auxiliary effects of plasticizers, flame retardant fuels, lubricants, and anti-aging agents, the fireproof PP recycled materials obtained have better flame retardant properties, mechanical properties, and low thermal conductivity. When the new energy products produced are used, the possibility of combustion and breakage is reduced, and their durability and safety of use are improved. In addition, the light weight reduces the energy loss of the car, which plays a better energy-saving role.

[0036] 2. Through the reaction of phosphate acrylate monomers, tris(2-hydroxyethyl)isocyanuric acid triacrylate, 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, and in combination with anhydride compatibilizers, the light flame retardant has a better compatibility-promoting effect, so that the prepared flame retardant has better flame retardancy, compatibility, insulation and toughness, and has the advantage of light weight. When the flame retardant is used in the production of fire-proof PP recycled materials, it can further improve the toughness, flame retardancy, insulation, and heat resistance of the fire-proof PP recycled materials, and make them lighter in weight. When used in the production of various accessories or auxiliary parts for new energy vehicles, it has a better synergistic effect, thereby reducing the possibility of breakage and combustion, while reducing energy loss. DETAILED DESCRIPTION

[0037] The present application is further described in detail below with reference to the embodiments.

[0038] Introduction of some raw materials: Table 1 Introduction of some raw materials Example

[0039] Example 1 A method for preparing fireproof PP recycled materials for new energy, which is prepared by the following method: Weigh 1.85 kg of flame retardant compatibilizer and heat it to 190°C, then add 5 kg of light flame retardant and stir at a speed of 30 r / min for 30 minutes to fully mix and solidify, and cool to 30°C, then put it into a grinder for crushing, sieve 500 mesh, and obtain flame retardant; Weigh 10kg of recycled material, 0.2kg of plasticizer, 3kg of flame retardant, 0.1kg of lubricant and 0.1kg of anti-aging agent and put them into a high-speed mixer. Mix them at a speed of 100r / min for 10min to make it fully uniform, and then transfer them to a twin-screw extruder for extrusion. The extruded material enters a cooling water tank for water cooling, and then passes through a drying device to dry the moisture, and then enters a granulator for granulation to obtain fire-resistant PP recycled material.

[0040] Among them, the flame retardant compatibilizer is maleic anhydride grafted PP, the lightweight flame retardant is porous silica aerogel, and the average particle size of the porous silica aerogel is 100nm; the plasticizer is 1,2-cyclohexanedicarboxylic acid diisopropyl ester; the lubricant is PE wax; and the anti-aging agent is antioxidant 168.

[0041] Table 2 Temperature settings of twin-screw extruder Temperature ℃ Zone 1 Zone 2 Zone 3 District 4 District 5 District 6 District 7 Die head set up 180 185 190 200 210 200 190 185 Example 2 The difference between Example 2 and Example 1 is that the combination or amount of raw materials is different, as follows: 2.2kg flame retardant compatibilizer, 5kg lightweight flame retardant; Recycled material 10kg, plasticizer 0.5kg, flame retardant 5.5kg, lubricant 0.3kg, anti-aging agent 0.15kg; Among them, the flame retardant compatibilizer is maleic anhydride grafted PP, the lightweight flame retardant is porous silica aerogel, and the average particle size of the porous silica aerogel is 300nm; the plasticizer is composed of 0.3kg 1,2-cyclohexanedicarboxylic acid diisopropyl ester and 0.2kg acetyl citrate tributyl ester; the lubricant is PE wax; the anti-aging agent is composed of 0.1kg antioxidant 1010 and 0.05kg UV-P.

[0042] Example 3 The difference between Example 3 and Example 1 is that the combination or amount of raw materials is different, as follows: 2.75kg flame retardant compatibilizer, 5kg lightweight flame retardant; Recycled material 10kg, plasticizer 0.8kg, flame retardant 8kg, lubricant 0.5kg, anti-aging agent 0.2kg; Among them, the flame retardant compatibilizer is maleic anhydride grafted PP, the lightweight flame retardant is zeolite powder, and the particle size of the zeolite powder is 2μm; the plasticizer is 1,2-cyclohexanedicarboxylic acid diisopropyl ester; the lubricant is PE wax; the anti-aging agent consists of 0.1kg antioxidant 168 and 0.1kg UV770.

[0043] Example 4 The difference between Example 4 and Example 2 is that the lightweight flame retardant is composed of 2kg expanded perlite powder and 3kg porous silica aerogel; wherein the particle size of the expanded perlite powder is 2μm, and the average particle size of the porous silica aerogel is 300nm.

[0044] Example 5 The difference between Example 5 and Example 2 is that the lightweight flame retardant is composed of 1 kg of expanded perlite powder, 3 kg of porous silica aerogel, and 1 kg of microporous calcium silicate; wherein the particle sizes of the expanded perlite powder and the microporous calcium silicate are both 2 μm, and the average particle size of the porous silica aerogel is 300 nm.

[0045] Example 6 The difference between Example 6 and Example 2 is that the lightweight flame retardant is composed of 1 kg expanded perlite powder, 2.5 kg porous silica aerogel, 0.5 kg microporous calcium silicate, and 1 kg zeolite powder; wherein the particle sizes of the expanded perlite powder and microporous calcium silicate are both 5 μm, the particle sizes of the zeolite powder are both 8 μm, and the average particle size of the porous silica aerogel is 200 nm.

[0046] Example 7 The difference between Example 7 and Example 2 is that the lightweight flame retardant is composed of 1.6 kg expanded perlite powder, 2.4 kg porous silica aerogel, 0.5 kg microporous calcium silicate, and 0.5 kg zeolite powder, the particle sizes of the expanded perlite powder, microporous calcium silicate, and zeolite powder are all 5 μm, and the average particle size of the porous silica aerogel is 100 nm.

[0047] Example 8 The difference between Example 8 and Example 6 is that the flame retardant compatibilizer is prepared by the following method: Weigh 1kg of phosphate acrylate monomer and 0.01kg of initiator into a reactor and stir for 10min at a speed of 50r / min to fully mix them. Heat to 65°C and react for 1h. Then add 0.5kg of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and continue stirring to fully mix them. React for 30min, then add 0.08kg of tris(2-hydroxyethyl)isocyanuric acid triacrylate and continue stirring to fully mix them. React for 20min, then add 2kg of maleic anhydride compatibilizer and 2kg of diluent and continue stirring to fully mix them. Adjust the pH value to 7, heat to 120°C at -0.1MPa, perform reduced pressure distillation, and solidify to obtain a flame retardant compatibilizer.

[0048] The phosphate ester acrylate monomer is 2-hydroxyethyl methacrylate phosphate; the maleic anhydride compatibilizer is maleic acid resin; the initiator is initiator BPO; and the diluent is N-methylpyrrolidone.

[0049] Example 9 The difference between Example 9 and Example 8 is that the amount and composition of the flame retardant compatibilizer are different, specifically as follows: 2 kg of phosphate acrylate monomer, 0.02 kg of initiator; 0.3 kg of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane; 0.2 kg of tris(2-hydroxyethyl)isocyanuric acid triacrylate; 3.8 kg of maleic anhydride compatibilizer, 5 kg of diluent.

[0050] The phosphate ester acrylate monomer is di(methacryloyloxyethyl) hydrogen phosphate; the maleic anhydride compatibilizer is maleic anhydride grafted PP.

[0051] Example 10 The difference between Example 10 and Example 8 is that the amount and composition of the flame retardant compatibilizer are different, specifically as follows: 3 kg of phosphate acrylate monomer, 0.03 kg of initiator; 0.1 kg of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane; 0.35 kg of tris(2-hydroxyethyl)isocyanuric acid triacrylate; 5 kg of maleic anhydride compatibilizer, 8 kg of diluent.

[0052] The phosphate ester acrylate monomer is alkyl acrylate phosphate; the maleic anhydride compatibilizer is maleic anhydride grafted SEBS.

[0053] Embodiment 11 The difference between Example 11 and Example 9 is that the phosphate ester acrylate monomer is composed of 1 kg of 2-hydroxyethyl methacrylate phosphate and 1 kg of di(methacryloyloxyethyl) hydrogen phosphate.

[0054] Example 12 The difference between Example 12 and Example 9 is that the phosphate ester acrylate monomers include 0.5 kg 2-hydroxyethyl methacrylate phosphate, 1 kg di(methacryloyloxyethyl) hydrogen phosphate, and 0.5 kg alkyl acrylate phosphate.

[0055] Example 13 The difference between Example 13 and Example 9 is that the phosphate ester acrylate monomers include 1.5 kg 2-hydroxyethyl methacrylate phosphate, 0.3 kg di(methacryloyloxyethyl) hydrogen phosphate, and 0.2 kg alkyl acrylate phosphate.

[0056] Embodiment 14 The difference between Example 14 and Example 12 is that the maleic anhydride compatibilizer consists of 0.8 kg of maleic acid resin and 3 kg of maleic anhydride grafted PP.

[0057] Embodiment 15 The difference between Example 15 and Example 12 is that the maleic anhydride compatibilizer consists of 1 kg of maleic acid resin, 2 kg of maleic anhydride grafted PP, and 0.8 kg of maleic anhydride grafted SEBS.

[0058] Example 16 The difference between Example 16 and Example 12 is that the maleic anhydride compatibilizer consists of 0.5 kg maleic acid resin, 2 kg maleic anhydride grafted PP, and 1.3 kg maleic anhydride grafted SEBS.

[0059] Embodiment 17 The difference between Example 17 and Example 8 is that tris(2-hydroxyethyl)isocyanurate triacrylate is replaced by 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane in an equal amount.

[0060] Embodiment 18 The difference between Example 18 and Example 8 is that 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane is replaced by tris(3-hydroxyethyl)isocyanurate triacrylate in an equal amount.

[0061] Embodiment 19 The difference between Example 19 and Example 8 is that the phosphate ester acrylate monomer is replaced by an equal amount of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane.

[0062] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the flame retardant material is antimony trioxide (with an average particle size of 100 nm).

[0063] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the lightweight flame retardant is antimony trioxide (with an average particle size of 100 nm).

[0064] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the lightweight flame retardant is silicon dioxide (with an average particle size of 100 nm).

[0065] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the lightweight flame retardant is flame retardant ABS (LG AF-303S from Korea), and the fourth zone and the fifth zone of the twin-screw extruder are set at 220° C. and 230° C., respectively.

[0066] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that: under the substrate of Comparative Example 4, the flame retardant compatibilizer is maleic anhydride grafted ABS (Hengtai Plastic Type ABS-g-MAH, grafting rate 1.2-04%).

[0067] Performance testing Detection method / test method The fireproof PP recycled materials and PP recycled materials obtained in Examples 1-19 and Comparative Examples 1-5 were injection molded into several test samples, and then the following performance tests were performed.

[0068] Notched impact strength: tested in accordance with ASTM D256-2006.

[0069] Flame retardant grade: tested according to UL-94 standard.

[0070] Oxygen index: Refer to GB / T 2406-93 to test the oxygen index.

[0071] CTI test: refer to GB / T 4207-2012.

[0072] In addition, the density of the fire-resistant PP recycled materials obtained in Examples 1-19 of the present application is 0.9 g / cm 3 The density of the comparative examples 1-5 is greater than 0.9 g / cm 3 .

[0073] The above experiment was tested 5 times and the average value was taken, as shown in Table 2; Table 2 Experimental data of Examples 1-19 and Comparative Examples 1-5 Combining Example 1 and Comparative Examples 1-5 and Table 1, it can be seen that the oxygen index, CTI value, and notched impact strength of Comparative Examples 1-5 are lower than those of Example 1, indicating that the flame retardant compatibilizer of the present application and the light flame retardant compound, the flame retardant obtained has better toughening and flame retardant effects, and has the advantages of light weight, etc. Therefore, it is used in PP recycled materials to play a better role in fire prevention and toughening, and when used in automotive interior parts, the shell of the charging pack of the car, and the shell of the energy storage battery of the car, it has better flame retardancy and impact toughness. Reduce the possibility of burning, breakage, etc., while meeting the "lightweight" concept of new energy vehicles and reducing the energy loss of new energy vehicles.

[0074] By comparing Example 2 with Example 6-7 and combining with Table 2, it can be seen that the oxygen index, CTI value and notched impact strength of Example 6-7 are higher than those of Example 2, indicating that the expanded perlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder of the present application are compounded in a weight ratio of (2-3.2): (4-4.8): 1: (1-2), which has a better synergistic effect, and is combined with a flame retardant compatibilizer to improve the fireproof performance and impact toughness of the obtained fireproof PP recycled material, reduce the possibility of breakage and combustion after being used in new energy vehicle accessories, and improve the safety of new energy vehicles.

[0075] By comparing Example 6 and Example 8 and combining with Table 2, it can be seen that the oxygen index, CTI value and notched impact strength of Example 8 are higher than those of Example 6, indicating that the flame retardant compatibilizer prepared by phosphate acrylate monomer, 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, tris(2-hydroxyethyl)isocyanuric acid triacrylate and maleic anhydride compatibilizer has good flame retardancy and compatibility, and is combined with expanded perlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder to obtain the obtained flame retardant material applied to the fireproof PP recycled raw material system to obtain better impact toughness and flame retardant effect.

[0076] By comparing Example 9 with Examples 12-13 and combining with Table 2, it can be seen that the oxygen index, CTI value, and notched impact strength of Examples 12-13 are higher than those of Example 9.

[0077] It is shown that when the weight ratio of 2-hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate is (1-7.5):(1-2.5):1 for compounding, a better synergistic effect is achieved, and a cross-linked macromolecular polymer is formed by further reacting with 1,3-bis(3-methacryloyloxypropyl)tetrakis(trimethylsiloxy)disiloxane and tris(2-hydroxyethyl)isocyanuric acid triacrylate.

[0078] In combination with maleic anhydride compatibilizer, the flame retardant compatibilizer has flame retardant performance, compatibility and toughening effect, which can further improve the compatibility of expanded pearlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder in the raw material system of fireproof PP recycled materials, so that the fireproof PP recycled materials have better fireproof performance and impact toughness. It can be used in new energy to play a better fireproof and burst resistance, and improve the safety of new energy accessories produced.

[0079] By comparing Examples 17-19 with Example 8 and combining with Table 2, it can be seen that the oxygen index, CTI value and notched impact strength of Example 8 are higher than those of Examples 17-19, indicating that the flame retardant compatibilizer prepared by using the phosphate acrylate monomer, 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, tris(2-hydroxyethyl)isocyanuric acid triacrylate and acid anhydride compatibilizer as main raw materials of the present application is applied to the fire-proof PP recycled raw material system, which plays a better synergistic role, thereby reducing the possibility of combustion and breakage.

[0080] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A fireproof PP recycled material for new energy, It is characterized in that The invention comprises the following raw materials in parts by weight: PP recycled material 100 pieces Plasticizer 2-8 parts Flame retardant 30-80 parts Lubricant 1-5 parts 1-2 parts of anti-aging agent; The flame retardant material is composed of a light flame retardant and a flame retardant compatibilizer in a weight ratio of 10: (3.7-5.5); The lightweight flame retardant is one or more of expanded pearlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder.

2. The fireproof PP recycled material for new energy according to claim 1, Features: The weight ratio of the expanded pearlite powder, porous silica aerogel, microporous calcium silicate and zeolite powder is (2-3.2): (4-4.8): 1: (1-2).

3. The fireproof PP recycled material for new energy according to claim 1, Features: The particle size of the porous silica aerogel is 100-300nm; the particle sizes of the expanded pearlite powder, microporous calcium silicate and zeolite powder are all 2-8µm.

4. The fireproof PP recycled material for new energy according to claim 1, It is characterized in that The flame retardant compatibilizer is prepared from the following raw materials in parts by weight: Phosphate acrylate monomer 1-3 parts Tris(2-hydroxyethyl)isocyanuric acid triacrylate 0.08-0.35 parts 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane 0.1-0.5 parts Maleic anhydride compatibilizer 2-5 parts Initiator 0.01-0.03 parts 3-8 parts of diluent.

5. The fireproof PP recycled material for new energy according to claim 4, Features: The phosphate ester acrylate monomer is one or more of 2-hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate.

6. The fireproof PP recycled material for new energy according to claim 5, Features: The weight ratio of the 2-hydroxyethyl methacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, and alkyl acrylate phosphate is (1-7.5):(1-2.5):

1.

7. The fireproof PP recycled material for new energy use according to claim 4, Features: The maleic anhydride compatibilizer is one or more of maleic acid resin, maleic anhydride grafted PP, and maleic anhydride grafted SEBS.

8. The fireproof PP recycled material for new energy use according to claim 7, Features: The weight ratio of the maleic acid resin, maleic anhydride grafted PP and maleic anhydride grafted SEBS is (0.5-1):2:(0.8-1.3).

9. The fireproof PP recycled material for new energy according to claim 1, Features: The antioxidant is one or more of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, antioxidant 168, UV770, UV-P, UV531, and UV-327; The lubricant is one or more of PETS, EBS, PE wax and triphenyl phosphate; The plasticizer is one or more of glyceryl tribenzoate, acetyl tributyl citrate, 1,2-cyclohexanedicarboxylic acid diisopropyl ester, and acetylated cyclohexanol acetyl ricinoleate.

10. A method for preparing fireproof PP recycled materials for new energy use as claimed in any one of claims 1 to 9, It is characterized in that Prepared by the following method: According to the weight percentage, the flame retardant compatibilizer is weighed and heated until it is melted, and then the light flame retardant is added and mixed evenly, cooled, crushed, and sieved to obtain a flame retardant material; According to weight parts, the recycled material, plasticizer, flame retardant, lubricant and anti-aging agent are weighed and mixed evenly, extruded, cooled and granulated to obtain fireproof PP recycled material.