Preparation process of EVA (Ethylene Vinyl Acetate) integrated foaming hot-press molding tray
Through the multi-step reaction preparation process of modified EVA resin and foaming agent, the problems of the pallet in flame retardant and corrosion protection were solved, and EVA integrated foaming hot-pressing pallet with excellent performance were prepared, which significantly improved its use quality .
Patent Information
- Application Number
- CN202410252710.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing pallets perform poorly in flame retardant and corrosion protection, affecting their use quality.
Modified EVA resin particles are heated and foamed with foaming agent, stabilizer and additives, and intermediates with flame retardant, water resistance, corrosion resistance and aging resistance are prepared through multiple reactions, to form modified EVA resin, and through heat Press forming process to prepare EVA integrated foaming hot press forming tray.
It significantly improves the flame retardant, corrosion-proof and aging resistance of the pallet, and improves its quality of use.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foaming and hot-pressing formed pallets, and in particular to a preparation process of an EVA integrated foaming and hot-pressing formed pallet. Background Art
[0002] Chinese patent CN112238665B discloses a pallet substrate and a preparation process thereof, wherein the pallet substrate comprises an intermediate base layer, elastic buffer layers arranged on both sides of the intermediate base layer, a support layer arranged on the elastic buffer layer, a surface protection layer arranged on the support layer, and the intermediate base layer, the elastic buffer layer, the support layer and the surface protection layer are multi-layer co-extruded, wherein the intermediate base layer is a PS base layer, the elastic buffer layer is an EVA base layer, the support layer is a PP base layer, and the surface protection layer is a PE base layer; In the prior art, a co-extruded pallet substrate is used to melt-combine an intermediate base layer, an elastic buffer layer, a support layer and a surface protection layer into a whole in a layered manner to meet the substrate requirements for hot pressing into a pallet. The hot pressing tensile fracture resistance is excellent, and it can provide impact buffering, surface contact protection, and frame structure strength. However, the flame retardant and corrosion resistant performance of the molded pallet is not ideal, which leads to a significant impact on the quality of the molded pallet during use. Summary of the invention
[0003] The purpose of the present invention is to provide a preparation process of an EVA integrated foaming hot-pressing molded tray to solve the following technical problem: the flame retardant and corrosion resistant performance of the molded tray is not ideal, which leads to a great impact on the quality of the molded tray during use.
[0004] The purpose of the present invention can be achieved by the following technical solutions: A preparation process of an EVA integrated foaming and hot-pressing molded tray comprises the following steps: The modified EVA resin particles, the foaming agent, the stabilizer and the additive raw materials are heated and foamed, heated, cooled and trimmed to obtain a foamed hot-pressed tray; The preparation process of the modified EVA resin comprises the following steps: Step 1: Carbazole and tetrahydrofuran are added to a flask, and then sodium hydride is added, stirred at room temperature for 30 minutes, and then the temperature is raised to 60°C, phosphorus oxychloride is added to the flask, and refluxed for 2-3 hours. After the reaction is completed, a saturated ammonium chloride solution is added to quench the reaction to obtain intermediate 1; Step 2: 3-fluoro-4-vinylphenol and ether were mixed, isopropanol-platinum was added, the temperature was raised to 90°C and stirred for reaction for 8 hours, and then tetramethylsilane was slowly added dropwise. After the addition was complete, the mixture was kept at a constant temperature for reaction for 24 hours to obtain intermediate 2; Step 3: Add intermediate 2, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 1, heat to 60°C, react for 5 hours, cool, and obtain intermediate 3; Step 4: Add EVA to xylene, stir in a 70°C water bath to dissolve EVA in xylene to form a homogeneous solution, then keep the temperature at 60°C, dropwise add a 0.5 mol / L sodium hydroxide-methanol solution, and react for 5-6 hours; then cool, filter, wash, dry, weigh, and finally obtain saponified EVA; Saponified EVA, acetone and anhydrous sodium carbonate were added into a flask, nitrogen was introduced, and the mixture was stirred for 1 hour. Then, intermediate 3 was added, the temperature was raised to 60° C., the mixture was reacted for 5 hours, and the mixture was cooled to obtain a modified EVA resin.
[0005] As a further solution of the present invention: in step 1, the dosage ratio of carbazole, tetrahydrofuran, sodium hydride and phosphorus oxychloride is controlled to be 1 mol: 200-400 mL: 2 mol: 0.01 mol.
[0006] As a further solution of the present invention: in step 2, the dosage ratio of 3-fluoro-4-vinylphenol, ether, isopropanol-platinum and tetramethylsilane is controlled to be 1 mol: 600-1000 mL: 0.1-0.2 mol: 1 mol.
[0007] As a further solution of the present invention: in step 3, the usage ratio of intermediate 2, acetone, anhydrous sodium carbonate and intermediate 1 is controlled to be 1 mol: 600-1000 mL: 50-70 g: 1 mol.
[0008] As a further solution of the present invention: in step 4, the dosage ratio of EVA, xylene and sodium hydroxide is controlled to be 1 g: 140-160 mL: 1.2-1.5 mol.
[0009] As a further solution of the present invention: in step 4, the dosage ratio of saponified EVA, acetone, anhydrous sodium carbonate and intermediate 3 is controlled to be 1 mol: 600-1000 mL: 50-70 g: 1 mol.
[0010] As a further solution of the present invention: in step 1, the raw materials are the following in parts by weight: 60-75 parts of modified EVA resin particles, 5-15 parts of foaming agent, 1-5 parts of stabilizer, and 5-10 parts of additives.
[0011] As a further solution of the present invention: the foaming agent is prepared by mixing one or more raw materials of sodium carbonate, sodium bicarbonate and zinc oxide in any proportion.
[0012] As a further solution of the present invention: the stabilizer is prepared by mixing one or more of lead stearate and dihydroxybenzophenone in any proportion.
[0013] As a further solution of the present invention: the additive is prepared by mixing the raw materials of phenol formaldehyde resin and epoxidized soybean oil in any proportion.
[0014] Beneficial effects of the present invention: In the present invention, in step 1, carbazole is reacted with an active chlorine of phosphorus oxychloride to obtain an intermediate 1 containing phosphorus and nitrogen flame retardants; in step 2, 3-fluoro-4-vinylphenol is reacted with tetramethylsilane to obtain an intermediate 2 containing siloxane bonds and CF bonds, so that the intermediate 2 has excellent properties such as water resistance, oil resistance, corrosion resistance, and aging resistance; in step 3, the hydroxyl group of the intermediate 2 is reacted with an active chlorine of the intermediate 1 to obtain an intermediate 3 having multiple properties of flame retardancy, water resistance, oil resistance, corrosion resistance, and aging resistance; in step 4, the graft modification of the EVA material is to utilize the acetyl group on its molecular chain, which is saponified with NaOH and then reacted with an active chlorine of the intermediate 3 to obtain a modified EVA resin, thereby effectively improving the multiple properties of the EVA resin such as flame retardancy, water resistance, oil resistance, corrosion resistance, and aging resistance; An EVA integrated foamed hot-pressed molded pallet is prepared based on modified EVA resin, so that the pallet has multiple properties such as flame retardancy, water and oil resistance, corrosion resistance, and aging resistance. DETAILED DESCRIPTION
[0015] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Example 1 The present invention is a preparation process of an EVA integrated foaming and hot pressing forming tray, comprising the following steps: S1, heating and foaming: preparing modified EVA resin particles, foaming agent, stabilizer and additive raw materials by weight, and mixing them evenly to form a foaming material, putting the foaming material into the hopper of a foaming machine, heating the foaming material through a preheater to make it reach a molten state, and the preheated foaming material enters the foaming chamber of the foaming machine, and the temperature and pressure are adjusted to generate a large number of bubbles, so that the foaming material expands and reduces the weight of the product; The raw materials in step S1 are as follows by weight: 60 parts of modified EVA resin particles, 5 parts of foaming agent, 1 part of stabilizer, and 5 parts of additives; the foaming agent is prepared by mixing one or more parts of sodium carbonate, sodium bicarbonate, and zinc oxide in any proportion; the stabilizer is prepared by mixing one or more parts of lead stearate and dihydroxybenzophenone in any proportion; the additive is prepared by mixing the raw materials of phenol formaldehyde resin and epoxidized soybean oil in any proportion; S2, hot pressing: adding the foamed material in step S1 into the tray mold and performing hot pressing molding at a hot pressing pressure of 8 MPaG; S3, heating: hot pressing, place the mold on the heating plate and continue heating at 150-180℃ for 8-15min until it is completely softened and fills the entire tray space; S4, cooling: take out the hot-pressed tray and put it into cold water for cooling. The temperature of the cold water is 15-20°C and the cooling time is 5-10 minutes to make it completely solidified; S5, trimming: After the tray is completely cooled and solidified, it is taken out and trimmed, such as trimming the edges, grinding, etc. Finally, it is packaged and delivered according to customer requirements; The preparation process of modified EVA resin comprises the following steps: Step 1: Carbazole and tetrahydrofuran are added to a flask, and then sodium hydride is added, stirred at room temperature for 30 minutes, and then the temperature is raised to 60°C, phosphorus oxychloride is added to the flask, and refluxed for 2-3 hours. After the reaction is completed, a saturated ammonium chloride solution is added to quench the reaction to obtain intermediate 1; The dosage ratio of carbazole, tetrahydrofuran, sodium hydride and phosphorus oxychloride is controlled to be 1 mol: 200 mL: 2 mol: 0.01 mol; Step 2: 3-fluoro-4-vinylphenol and ether were mixed, isopropanol-platinum was added thereto, the temperature was raised to 90°C and stirred for reaction for 8 hours, and then tetramethylsilane was slowly added dropwise thereto. After the addition was complete, the mixture was kept at a constant temperature for reaction for 24 hours to obtain intermediate 2; The dosage ratio of 3-fluoro-4-vinylphenol, ether, isopropanol-platinum and tetramethylsilane was controlled to be 1 mol: 600 mL: 0.1 mol: 1 mol; Step 3: Add intermediate 2, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 1, heat to 60°C, react for 5 hours, cool, and obtain intermediate 3; The dosage ratio of intermediate 2, acetone, anhydrous sodium carbonate and intermediate 1 is controlled to be 1 mol: 600 mL: 50 g: 1 mol; Step 4: Add EVA to xylene, stir in a 70°C water bath to dissolve EVA in xylene to form a homogeneous solution, then keep the temperature at 60°C, dropwise add a 0.5 mol / L sodium hydroxide-methanol solution, and react for 5-6 hours; then cool, filter, wash, dry, weigh, and finally obtain saponified EVA; The dosage ratio of EVA, xylene and sodium hydroxide was controlled to be 1 g: 140 mL: 1.2 mol; Add saponified EVA, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 3, heat to 60°C, react for 5 hours, cool, and obtain modified EVA resin; The dosage ratio of saponified EVA, acetone, anhydrous sodium carbonate and intermediate 3 is controlled to be 1 mol: 600 mL: 50 g: 1 mol.
[0017] Example 2 The present invention is a preparation process of an EVA integrated foaming and hot pressing forming tray, comprising the following steps: S1, heating and foaming: preparing modified EVA resin particles, foaming agent, stabilizer and additive raw materials by weight, and mixing them evenly to form a foaming material, putting the foaming material into the hopper of a foaming machine, heating the foaming material through a preheater to make it reach a molten state, and the preheated foaming material enters the foaming chamber of the foaming machine, and the temperature and pressure are adjusted to generate a large number of bubbles, so that the foaming material expands and reduces the weight of the product; The raw materials in step S1 are as follows by weight: 70 parts of modified EVA resin particles, 10 parts of foaming agent, 3 parts of stabilizer, and 8 parts of additive; the foaming agent is prepared by mixing one or more parts of sodium carbonate, sodium bicarbonate, and zinc oxide in any proportion; the stabilizer is prepared by mixing one or more parts of lead stearate and dihydroxybenzophenone in any proportion; the additive is prepared by mixing the raw materials of phenol formaldehyde resin and epoxidized soybean oil in any proportion; S2, hot pressing: adding the foamed material in step S1 into the tray mold and performing hot pressing molding at a hot pressing pressure of 9 MPaG; S3, heating: hot pressing, place the mold on the heating plate and continue heating at 150-180℃ for 8-15min until it is completely softened and fills the entire tray space; S4, cooling: take out the hot-pressed tray and put it into cold water for cooling. The temperature of the cold water is 15-20°C and the cooling time is 5-10 minutes to make it completely solidified; S5, trimming: After the tray is completely cooled and solidified, it is taken out and trimmed, such as trimming the edges, grinding, etc. Finally, it is packaged and delivered according to customer requirements; The preparation process of modified EVA resin comprises the following steps: Step 1: Carbazole and tetrahydrofuran are added to a flask, and then sodium hydride is added, stirred at room temperature for 30 minutes, and then the temperature is raised to 60°C, phosphorus oxychloride is added to the flask, and refluxed for 2-3 hours. After the reaction is completed, a saturated ammonium chloride solution is added to quench the reaction to obtain intermediate 1; The dosage ratio of carbazole, tetrahydrofuran, sodium hydride and phosphorus oxychloride is controlled to be 1 mol: 400 mL: 2 mol: 0.01 mol; Step 2: 3-fluoro-4-vinylphenol and ether were mixed, isopropanol-platinum was added thereto, the temperature was raised to 90°C and stirred for reaction for 8 hours, and then tetramethylsilane was slowly added dropwise thereto. After the addition was complete, the mixture was kept at a constant temperature for reaction for 24 hours to obtain intermediate 2; The dosage ratio of 3-fluoro-4-vinylphenol, ether, isopropanol-platinum and tetramethylsilane is controlled to be 1 mol: 1000 mL: 0.2 mol: 1 mol; Step 3: Add intermediate 2, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 1, heat to 60°C, react for 5 hours, cool, and obtain intermediate 3; The dosage ratio of intermediate 2, acetone, anhydrous sodium carbonate and intermediate 1 is controlled to be 1 mol: 1000 mL: 70 g: 1 mol; Step 4: Add EVA to xylene, stir in a 70°C water bath to dissolve EVA in xylene to form a homogeneous solution, then keep the temperature at 60°C, dropwise add a 0.5 mol / L sodium hydroxide-methanol solution, and react for 5-6 hours; then cool, filter, wash, dry, weigh, and finally obtain saponified EVA; The dosage ratio of EVA, xylene and sodium hydroxide was controlled to be 1 g: 160 mL: 1.5 mol; Add saponified EVA, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 3, heat to 60°C, react for 5 hours, cool, and obtain modified EVA resin; The dosage ratio of saponified EVA, acetone, anhydrous sodium carbonate and intermediate 3 is controlled to be 1 mol: 1000 mL: 70 g: 1 mol.
[0018] Example 3 The present invention is a preparation process of an EVA integrated foaming and hot pressing forming tray, comprising the following steps: S1, heating and foaming: preparing modified EVA resin particles, foaming agent, stabilizer and additive raw materials by weight, and mixing them evenly to form a foaming material, putting the foaming material into the hopper of a foaming machine, heating the foaming material through a preheater to make it reach a molten state, and the preheated foaming material enters the foaming chamber of the foaming machine, and the temperature and pressure are adjusted to generate a large number of bubbles, so that the foaming material expands and reduces the weight of the product; The raw materials in step S1 are as follows by weight: 75 parts of modified EVA resin particles, 15 parts of foaming agent, 5 parts of stabilizer, and 10 parts of additives; the foaming agent is prepared by mixing one or more parts of sodium carbonate, sodium bicarbonate, and zinc oxide in any proportion; the stabilizer is prepared by mixing one or more parts of lead stearate and dihydroxybenzophenone in any proportion; the additive is prepared by mixing the raw materials of phenol formaldehyde resin and epoxidized soybean oil in any proportion; S2, hot pressing: adding the foamed material in step S1 into the tray mold and hot pressing the material at a pressure of 10 MPaG; S3, heating: hot pressing, place the mold on the heating plate and continue heating at 150-180℃ for 8-15min until it is completely softened and fills the entire tray space; S4, cooling: take out the hot-pressed tray and put it into cold water for cooling. The temperature of the cold water is 15-20°C and the cooling time is 5-10 minutes to make it completely solidified; S5, trimming: After the tray is completely cooled and solidified, it is taken out and trimmed, such as trimming the edges, grinding, etc. Finally, it is packaged and delivered according to customer requirements; The preparation process of modified EVA resin comprises the following steps: Step 1: Carbazole and tetrahydrofuran are added to a flask, and then sodium hydride is added, stirred at room temperature for 30 minutes, and then the temperature is raised to 60°C, phosphorus oxychloride is added to the flask, and refluxed for 2-3 hours. After the reaction is completed, a saturated ammonium chloride solution is added to quench the reaction to obtain intermediate 1; The dosage ratio of carbazole, tetrahydrofuran, sodium hydride and phosphorus oxychloride is controlled to be 1 mol: 400 mL: 2 mol: 0.01 mol; Step 2: 3-fluoro-4-vinylphenol and ether were mixed, isopropanol-platinum was added thereto, the temperature was raised to 90°C and stirred for reaction for 8 hours, and then tetramethylsilane was slowly added dropwise thereto. After the addition was complete, the mixture was kept at a constant temperature for reaction for 24 hours to obtain intermediate 2; The dosage ratio of 3-fluoro-4-vinylphenol, ether, isopropanol-platinum and tetramethylsilane is controlled to be 1 mol: 1000 mL: 0.2 mol: 1 mol; Step 3: Add intermediate 2, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 1, heat to 60°C, react for 5 hours, cool, and obtain intermediate 3; The dosage ratio of intermediate 2, acetone, anhydrous sodium carbonate and intermediate 1 is controlled to be 1 mol: 1000 mL: 70 g: 1 mol; Step 4: Add EVA to xylene, stir in a 70°C water bath to dissolve EVA in xylene to form a homogeneous solution, then keep the temperature at 60°C, dropwise add a 0.5 mol / L sodium hydroxide-methanol solution, and react for 5-6 hours; then cool, filter, wash, dry, weigh, and finally obtain saponified EVA; The dosage ratio of EVA, xylene and sodium hydroxide was controlled to be 1 g: 160 mL: 1.5 mol; Add saponified EVA, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 3, heat to 60°C, react for 5 hours, cool, and obtain modified EVA resin; The dosage ratio of saponified EVA, acetone, anhydrous sodium carbonate and intermediate 3 is controlled to be 1 mol: 1000 mL: 70 g: 1 mol.
[0019] Comparative Example 1 The pallet obtained by the preparation process of Comparative Example 1 is different from that of Example 1 in that the modified EVA resin particles in S1 of Example 1 are replaced by EVA resin particles; Performance Testing The pallet samples obtained in Examples 1-3 and Comparative Example 1 were subjected to flame retardancy tests, specifically: using a COI oxygen index combustion tester from Motis to test the limiting oxygen index (LOI) according to standard GB / T2406.1-2008; The flame retardant test was performed on the pallet samples obtained in Examples 1-3 and Comparative Example 1, specifically: prepare several 100mL beakers, add 50mL of 0.1mol / L sulfuric acid solution to each beaker for standby use. Place the sample in the sulfuric acid solution, then seal each beaker with plastic wrap, and finally place the beaker in a 20°C constant temperature curing box for 48 hours of insulation treatment. After the sample has been acid-corroded for 48 hours, take the pallet sample out of the solution and place it in a 105°C forced air drying oven for drying for 2 hours, and then test the tensile yield strength of the corroded pallet sample; see the table below for details; It can be seen from the above table that the EVA integrated foaming and hot-pressing molded pallet prepared by the modified EVA resin in the present invention has good flame retardant and anti-corrosion properties.
[0020] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A preparation process of an EVA integrated foaming hot pressing molded tray, It is characterized in that The following steps are involved: The modified EVA resin particles, the foaming agent, the stabilizer and the additive raw materials are heated and foamed, heated, cooled and trimmed to obtain a foamed hot-pressed tray; The preparation process of the modified EVA resin comprises the following steps: Step 1: Carbazole and tetrahydrofuran are added to a flask, and then sodium hydride is added, stirred at room temperature for 30 minutes, and then the temperature is raised to 60°C, phosphorus oxychloride is added to the flask, and refluxed for 2-3 hours. After the reaction is completed, a saturated ammonium chloride solution is added to quench the reaction to obtain intermediate 1; Step 2: 3-fluoro-4-vinylphenol and ether were mixed, isopropanol-platinum was added, the temperature was raised to 90°C and stirred for reaction for 8 hours, and then tetramethylsilane was slowly added dropwise. After the addition was complete, the mixture was kept at a constant temperature for reaction for 24 hours to obtain intermediate 2; Step 3: Add intermediate 2, acetone and anhydrous sodium carbonate into a flask, introduce nitrogen, stir for 1 hour, then add intermediate 1, heat to 60°C, react for 5 hours, cool, and obtain intermediate 3; Step 4: Add EVA to xylene, stir in a 70°C water bath to dissolve EVA in xylene to form a homogeneous solution, then keep the temperature at 60°C, dropwise add a 0.5 mol / L sodium hydroxide-methanol solution, and react for 5-6 hours; then cool, filter, wash, dry, weigh, and finally obtain saponified EVA; Saponified EVA, acetone and anhydrous sodium carbonate were added into a flask, nitrogen was introduced, and the mixture was stirred for 1 hour. Then, intermediate 3 was added, the temperature was raised to 60° C., the mixture was reacted for 5 hours, and the mixture was cooled to obtain a modified EVA resin.
2. A process for preparing an EVA integrated foaming and hot pressing molded tray according to claim 1, It is characterized in that In step 1, the dosage ratio of carbazole, tetrahydrofuran, sodium hydride and phosphorus oxychloride is controlled to be 1 mol: 200-400 mL: 2 mol: 0.01 mol.
3. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that In step 2, the dosage ratio of 3-fluoro-4-vinylphenol, ether, isopropanol-platinum and tetramethylsilane is controlled to be 1 mol: 600-1000 mL: 0.1-0.2 mol: 1 mol.
4. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that In step 3, the usage ratio of intermediate 2, acetone, anhydrous sodium carbonate and intermediate 1 is controlled to be 1 mol: 600-1000 mL: 50-70 g: 1 mol.
5. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that In step 4, the dosage ratio of EVA, xylene and sodium hydroxide is controlled to be 1 g: 140-160 mL: 1.2-1.5 mol.
6. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that In step 4, the dosage ratio of saponified EVA, acetone, anhydrous sodium carbonate and intermediate 3 is controlled to be 1 mol: 600-1000 mL: 50-70 g: 1 mol.
7. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that In step 1, the raw materials are as follows in parts by weight: 60-75 parts of modified EVA resin particles, 5-15 parts of foaming agent, 1-5 parts of stabilizer, and 5-10 parts of additives.
8. The preparation process of the EVA integrated foaming and hot pressing molded tray according to claim 1, It is characterized in that The foaming agent is prepared by mixing one or more raw materials of sodium carbonate, sodium bicarbonate and zinc oxide in any proportion.
9. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that The stabilizer is prepared by mixing one or more parts of lead stearate and dihydroxybenzophenone in any proportion.
10. The preparation process of the EVA integrated foaming and hot pressing forming tray according to claim 1, It is characterized in that The additive is prepared by mixing raw materials of phenol formaldehyde resin and epoxidized soybean oil in any proportion.
Citation Information
Patent Citations
Biological phenol organic silicon resin as well as preparation method and applications thereof
CN110628027A
Flame-retardant wear-resistant plastic particle and processing technology thereof