Lip piece formula for enhancing wear resistance of lip and production process of lip piece formula
By adding glass fiber, molybdenum disulfide and modified carbon nanotubes to the PTFE lip sheet material, combined with the preparation and segmented sintering process of modified carbon nanotubes, the wear resistance and mechanical properties of PTFE lip sheet material are solved. Problem, achieving higher wear resistance and service life.
Patent Information
- Application Number
- CN202411079554.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing PTFE lip sheet materials have problems such as poor resilience, poor self-lubricity and poor wear resistance, resulting in short service life, poor seal reliability and high maintenance costs.
Using lip sheet formulas including PTFE, glass fiber, molybdenum disulfide and modified carbon nanotubes, the material's wear resistance and mechanical properties are improved through the preparation and segmented sintering process of modified carbon nanotubes.
It significantly improves the wear resistance and overall strength of the lip material, extends the service life, reduces maintenance costs, and is suitable for large-scale production.
Smart Images

Figure BDA0004983314370000081 
Figure BDA0004983314370000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a lip sheet formula for enhancing the wear resistance of a lip and a production process thereof. Background Art
[0002] In various machines, seals are used to prevent fluids or solid particles from leaking from adjacent joint surfaces of parts, and to prevent external impurities such as dust, air, and moisture from invading the device. Therefore, the material selection of seals is crucial for machinery. Polytetrafluoroethylene (PTFE) has excellent high and low temperature resistance and chemical corrosion resistance. Almost all strong acids, strong alkalis, strong oxidants, and salts have no effect on polytetrafluoroethylene. Based on this excellent performance, polytetrafluoroethylene is mostly used as a seal material in the existing technology.
[0003] The PTFE lip material is formed by mechanical drawing of polytetrafluoroethylene discs. It is drawn into a trumpet shape during processing. The PTFE material uses the size memory effect. The friction heat generated during work causes the lip to shrink continuously. Without the help of a spring, the lip can hold the rotating shaft tightly to avoid gaps between it and the shaft surface, and can compensate for wear and improve the sealing life and reliability. The PTFE oil seal lip material is a key factor in determining the sealing performance of the polytetrafluoroethylene oil seal. It determines the working temperature range, friction, wear performance, medium resistance and sealing performance of the polytetrafluoroethylene oil seal. However, the existing PTFE lip material still has the problems of poor resilience, poor self-lubrication and poor wear resistance, which seriously affect its service life and sealing reliability. The poor wear resistance leads to poor sliding lubrication when the lip contacts the rotating shaft, causing serious wear on the shaft and a short product life. In addition, due to the poor resilience of the polytetrafluoroethylene oil seal lip, the sealing lip has poor followability to the rotating shaft, which causes the lubricating oil to leak quickly, thereby increasing the maintenance cost and limiting its application in actual production.
[0004] Therefore, how to improve the elasticity, flexibility and wear resistance of PTFE lip materials is a technical problem that needs to be solved urgently. Summary of the invention
[0005] In order to improve the wear resistance of PTFE lip material, the present invention provides a lip formula and a production process for enhancing the wear resistance of the lip.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] The first aspect of the present invention provides a lip sheet formula for enhancing the wear resistance of the lip, which comprises the following raw materials in parts by weight:
[0008] PTFE 70-80 parts;
[0009] Glass fiber 10-15 parts;
[0010] 3-5 parts of molybdenum disulfide;
[0011] 1-3 parts of talcum powder;
[0012] 1-5 parts of modified carbon nanotubes;
[0013] The modified carbon nanotubes are prepared by the following steps:
[0014] Add carboxylated carbon nanotubes to thionyl chloride and N,N-dimethylformamide, reflux and stir at 70-75°C for 22-24 hours, evaporate at normal pressure, cool to room temperature, heat to 100°C, evacuate and then introduce argon to restore normal pressure, add dodecylamine, reflux and stir at 90-92°C for 5-6 hours, cool, filter, wash, and vacuum dry to obtain modified carbon nanotubes.
[0015] As a further embodiment of the present invention, the usage ratio of carboxylated carbon nanotubes, thionyl chloride, N,N-dimethylformamide and dodecylamine is 0.5-0.6 g:95 mL:0.5 mL:10-10.5 g.
[0016] As a further solution of the present invention, the carboxylated carbon nanotubes are prepared by the following steps:
[0017] The carbon nanotubes were added into concentrated nitric acid, heated and refluxed with stirring, cooled to room temperature, washed to neutrality, and dried to obtain carboxylated carbon nanotubes; wherein the amount ratio of the carbon nanotubes to the concentrated nitric acid was 3 g:12 mL.
[0018] As a further solution of the present invention, the particle size of the carbon nanotubes is 30-50 nm.
[0019] As a further solution of the present invention, the glass fiber has a diameter of 14-16 μm and a length of 120-150 μm.
[0020] As a further solution of the present invention, the particle size of the molybdenum disulfide is 120-180 μm.
[0021] A second aspect of the present invention provides a production process for a lip sheet formulation for enhancing the wear resistance of a lip, comprising the following steps:
[0022] Step 1: refrigerate PTFE, glass fiber, molybdenum disulfide, talcum powder and modified carbon nanotubes respectively, add them into a high-speed mixer according to weight parts, stir them evenly, and then dry, crush and sieve them in sequence to obtain crushed materials;
[0023] Step 2: The crushed materials are pressed and sintered in stages in sequence to obtain the product.
[0024] As a further solution of the present invention, the refrigeration temperature is ≤-20°C and the refrigeration time is 24-36h.
[0025] As a further solution of the present invention, the process steps of the segmented sintering are as follows:
[0026] Heating from room temperature to 180°C at a rate of 20-25°C / 10min;
[0027] From 180℃ to 290℃, the heating rate is 10-15℃ / 10min;
[0028] Heat from 290℃ to 330℃ at a rate of 3-5℃ / 10min, and keep at 330℃ for 90-100min;
[0029] Heat from 330°C to 375°C at a rate of 3-5°C / 10min, and keep at 375°C for 180-200min.
[0030] Beneficial effects of the present invention:
[0031] The present invention provides a lip sheet formula for enhancing the wear resistance of the lip and a production process thereof, wherein the lip sheet formula comprises the following raw materials: PTFE, glass fiber, molybdenum disulfide, talcum powder and modified carbon nanotubes, wherein molybdenum disulfide has good lubrication performance, and glass fiber has good mechanical property modification effect, and can cooperate with modified carbon nanotubes and molybdenum disulfide to improve the wear resistance and mechanical properties of polytetrafluoroethylene. Meanwhile, in the production process, low temperature refrigeration controls the powder to be stirred evenly, and sieving can better control the powder size, thereby improving the wear resistance of the product.
[0032] In the present invention, the modified carbon nanotubes are first carboxylated with concentrated nitric acid, and then the carboxyl groups are chlorinated and reacted with dodecylamine to form aliphatic alkylamide-modified carbon nanotubes, which improve the dispersibility and compatibility of the carbon nanotubes in the polymer, so that the composite material is mixed more evenly, and the good compatibility and mechanical strength can make the stress transmission effect more efficient, avoid stress concentration, and further improve the wear resistance of the composite material. In addition, the surface of the modified carbon nanotubes is grafted with long-chain molecules, which can form a certain mesh structure in the polytetrafluoroethylene material, and entangled on the molecular chain of polytetrafluoroethylene, so that the peeling and shedding effect of the wafer during the friction process is weakened, thereby improving the wear resistance of the composite material, and at the same time, the stress transmission effect with polytetrafluoroethylene is good, the pulling effect is obvious, and the tensile strength of the composite material is improved. On the other hand, the addition of the modified carbon nanotubes can play a role as a skeleton in the polytetrafluoroethylene material, and the modified carbon nanotubes are enriched on the surface in the initial wear stage, and the exposed modified carbon nanotubes bear part of the load, thereby further reducing the wear rate of the polytetrafluoroethylene material and improving the wear resistance of the polytetrafluoroethylene.
[0033] The present invention provides a lip piece formula for enhancing the wear resistance of the lip and a production process thereof. The raw materials of each component are appropriately proportioned, and the prepared lip piece material has excellent wear resistance and high overall strength. The production process is simple to operate, easy to implement, and suitable for large-scale production. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The carboxylated carbon nanotubes used in the examples and comparative examples of the present invention are prepared by the following steps:
[0036] 3 g of carbon nanotubes (particle size of 50 nm) were added to 12 mL of concentrated nitric acid, refluxed and stirred at 120° C. for 12-14 h, cooled to room temperature, washed with deionized water until neutral, and dried in a vacuum drying oven at 70° C. for 24 h to obtain carboxylated carbon nanotubes.
[0037] The polytetrafluoroethylene used in the present invention is Japanese Daikin PTFE M-111.
[0038] Example 1
[0039] This embodiment provides a modified carbon nanotube, which is prepared by the following steps:
[0040] 0.5 g of carboxylated carbon nanotubes were added to 95 mL of thionyl chloride and 0.5 mL of N,N-dimethylformamide, refluxed and stirred at 70 ° C for 24 h, evaporated at normal pressure, cooled to room temperature, heated to 100 ° C, evacuated, and then argon was introduced to restore normal pressure, 10 g of dodecylamine was added, refluxed and stirred at 90 ° C for 5 h, cooled to room temperature, diluted, filtered and washed 3 times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ° C for 24 h to obtain modified carbon nanotubes.
[0041] Example 2
[0042] This embodiment provides a modified carbon nanotube, which is prepared by the following steps:
[0043] 0.55 g of carboxylated carbon nanotubes were added to 95 mL of thionyl chloride and 0.5 mL of N,N-dimethylformamide, refluxed and stirred at 70 ° C for 24 h, evaporated at normal pressure, cooled to room temperature, heated to 100 ° C, evacuated, and then argon was introduced to restore normal pressure, 10.25 g of dodecylamine was added, refluxed and stirred at 90 ° C for 5 h, cooled to room temperature, diluted, filtered and washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ° C for 24 h to obtain modified carbon nanotubes.
[0044] Example 3
[0045] This embodiment provides a modified carbon nanotube, which is prepared by the following steps:
[0046] 0.6 g of carboxylated carbon nanotubes were added to 95 mL of thionyl chloride and 0.5 mL of N,N-dimethylformamide, refluxed and stirred at 70 ° C for 24 h, evaporated at normal pressure, cooled to room temperature, heated to 100 ° C, evacuated, and then argon was introduced to restore normal pressure, 10.5 g of dodecylamine was added, refluxed and stirred at 90 ° C for 5 h, cooled to room temperature, diluted, filtered and washed three times with anhydrous ethanol, and dried in a vacuum drying oven at 60 ° C for 24 h to obtain modified carbon nanotubes.
[0047] Comparative Example 1
[0048] In this comparative example, commercially available carbon nanotubes (50 nm) were directly used as modified carbon nanotubes.
[0049] Example 4
[0050] This embodiment provides a lip sheet formula and a production process for enhancing the wear resistance of the lip:
[0051] A lip sheet formula for enhancing the wear resistance of the lip, comprising the following raw materials in parts by weight:
[0052] PTFE 70 parts, glass fiber (diameter 14 μm, length 120 μm) 10 parts, molybdenum disulfide (particle size 120 μm) 4 parts, talc 2 parts, modified carbon nanotubes in Example 1 1 part;
[0053] The preparation steps are as follows:
[0054] Step 1: refrigerate PTFE, glass fiber, molybdenum disulfide, talcum powder and modified carbon nanotubes respectively at a temperature of ≤-20°C for 26 hours, add them into a high-speed mixer according to weight portions, stir them uniformly, and then dry, crush and sieve them in sequence to obtain a crushed material;
[0055] Step 2: Press and sinter the crushed materials in sequence, wherein the process steps of the segmented sintering are: heat up from room temperature to 180°C at a heating rate of 20°C / 10min; heat up from 180°C to 290°C at a heating rate of 10°C / 10min; heat up from 290°C to 330°C at a heating rate of 3°C / 10min, and keep at 330°C for 90min; heat up from 330°C to 375°C at a heating rate of 3°C / 10min, and keep at 375°C for 180min.
[0056] Example 5
[0057] The only difference from Example 4 is that:
[0058] One part of the modified carbon nanotubes in Example 1 was replaced with three parts of the modified carbon nanotubes in Example 2.
[0059] Example 6
[0060] The only difference from Example 4 is that:
[0061] One part of the modified carbon nanotubes in Example 1 was replaced with five parts of the modified carbon nanotubes in Example 3.
[0062] Example 7
[0063] The only difference from Example 4 is that:
[0064] A lip sheet formula for enhancing the wear resistance of the lip, comprising the following raw materials in parts by weight:
[0065] 75 parts of PTFE, 10 parts of glass fiber (diameter: 14 μm, length: 140 μm), 4 parts of molybdenum disulfide (particle size: 160 μm), 2 parts of talc powder, and 2 parts of the modified carbon nanotubes in Example 1.
[0066] Example 8
[0067] The only difference from Example 4 is that:
[0068] A lip sheet formula for enhancing the wear resistance of the lip, comprising the following raw materials in parts by weight:
[0069] 80 parts of PTFE, 12 parts of glass fiber (diameter: 16 μm, length: 150 μm), 4 parts of molybdenum disulfide (particle size: 140 μm), 3 parts of talc powder, and 3 parts of the modified carbon nanotubes in Example 1.
[0070] Example 9
[0071] The only difference from Example 4 is that:
[0072] Step 2: Press and sinter the crushed materials in sequence, wherein the process steps of the segmented sintering are: heat up from room temperature to 180°C at a heating rate of 25°C / 10min; heat up from 180°C to 290°C at a heating rate of 15°C / 10min; heat up from 290°C to 330°C at a heating rate of 5°C / 10min, and keep at 330°C for 100min; heat up from 330°C to 375°C at a heating rate of 5°C / 10min, and keep at 375°C for 180min.
[0073] Comparative Example 2
[0074] The only difference from Example 4 is that:
[0075] The modified carbon nanotubes in Example 1 are replaced by the modified carbon nanotubes in Comparative Example 1 while keeping the same amount.
[0076] Comparative Example 3
[0077] The only difference from Example 4 is that:
[0078] One part of the modified carbon nanotubes in Example 1 was replaced with 0.5 parts of the modified carbon nanotubes in Example 1.
[0079] Comparative Example 4
[0080] The only difference from Example 4 is that:
[0081] One part of the modified carbon nanotubes in Example 1 was replaced with 6 parts of the modified carbon nanotubes in Example 1.
[0082] Comparative Example 5
[0083] The only difference from Example 4 is that:
[0084] A lip sheet formula for enhancing the wear resistance of the lip, comprising the following raw materials in parts by weight:
[0085] 60 parts of PTFE, 8 parts of glass fiber (diameter: 14 μm, length: 140 μm), 4 parts of molybdenum disulfide (particle size: 160 μm), 2 parts of talc powder, and 2 parts of the modified carbon nanotubes in Example 1.
[0086] Comparative Example 6
[0087] The only difference from Example 4 is that:
[0088] A lip sheet formula for enhancing the wear resistance of the lip, comprising the following raw materials in parts by weight:
[0089] 95 parts of PTFE, 18 parts of glass fiber (diameter: 14 μm, length: 140 μm), 3 parts of molybdenum disulfide (particle size: 160 μm), 0.5 parts of talc powder, and 2 parts of the modified carbon nanotubes in Example 1.
[0090] Comparative Example 7
[0091] The only difference from Example 4 is that:
[0092] Step 2: Press and sinter the crushed materials in sequence, wherein the process steps of the segmented sintering are: heat up from room temperature to 180°C at a heating rate of 30°C / 10min; heat up from 180°C to 290°C at a heating rate of 10°C / 10min; heat up from 290°C to 330°C at a heating rate of 10°C / 10min, and keep at 330°C for 100min; heat up from 330°C to 375°C at a heating rate of 8°C / 10min, and keep at 375°C for 180min.
[0093] The following performance tests were conducted on Examples 4 to 9 and Comparative Examples 2 to 7: (1) The tensile strength and elongation at break of the obtained formula materials were tested in accordance with the provisions of GB / T 1040.2. (2) The lip sheet formulas in the Examples and Comparative Examples were prepared into lip sheet materials, and processed into specimens with a size of 20 mm×12 mm×4 mm. The wear resistance of the surface layer was tested by a friction and wear test. The counterpart was a GCr15 steel ball with a diameter of 6 mm and a hardness of 63 HRC. The load was 10 N, the sliding speed was 0.08 m / s, and the sliding distance was 600 m. The wear rate test results were measured and calculated as shown in Table 1:
[0094] Table 1
[0095]
[0096]
[0097] It can be seen from Table 1 that, compared with Comparative Examples 2-7, the lip materials obtained in Examples 4-9 have excellent mechanical properties, low wear loss, and good wear resistance. The carbon nanotubes added in Comparative Example 2 have not been modified, and their tensile strength and elongation at break are lower than those in Example 4. It can be seen that the unmodified carbon nanotubes have poor dispersion properties and poor compatibility with polytetrafluoroethylene, which makes the composite material mixed unevenly, thereby affecting the mechanical properties and wear resistance of the composite material. It can be seen from the data in Comparative Examples 3-7 that the amount of each raw material in the formula exceeds the range in the formula and the process is different, which will affect the mechanical properties and wear resistance of the lip material. In summary, the lip formula for enhancing the wear resistance of the lip provided by the present invention has an appropriate ratio of raw materials of each component, and the prepared lip material has excellent wear resistance and mechanical properties, and the production process is simple to operate, easy to implement, and suitable for large-scale production.
[0098] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0099] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A lip sheet formula for enhancing the wear resistance of the lip, characterized in that: It includes the following raw materials in parts by weight: PTFE 70-80 parts; Glass fiber 10-15 parts; 3-5 parts of molybdenum disulfide; 1-3 parts of talcum powder; 1-5 parts of modified carbon nanotubes; The modified carbon nanotubes are prepared by the following steps: Add carboxylated carbon nanotubes to thionyl chloride and N,N-dimethylformamide, reflux and stir at 70-75°C for 22-24 hours, evaporate at normal pressure, cool to room temperature, heat to 100°C, evacuate and then introduce argon to restore normal pressure, add dodecylamine, reflux and stir at 90-92°C for 5-6 hours, cool, filter, wash, and vacuum dry to obtain modified carbon nanotubes.
2. A lip sheet formulation for enhancing lip wear resistance according to claim 1, characterized in that: The usage ratio of carboxylated carbon nanotubes, thionyl chloride, N,N-dimethylformamide and dodecylamine is 0.5-0.6 g: 95 mL: 0.5 mL: 10-10.5 g.
3. The lip sheet formula for enhancing the wear resistance of the lip according to claim 1, characterized in that: The carboxylated carbon nanotubes are prepared by the following steps: The carbon nanotubes were added into concentrated nitric acid, heated and refluxed with stirring, cooled to room temperature, washed to neutrality, and dried to obtain carboxylated carbon nanotubes; wherein the amount ratio of the carbon nanotubes to the concentrated nitric acid was 3 g:12 mL.
4. A lip sheet formulation for enhancing lip wear resistance according to claim 3, characterized in that: The particle size of the carbon nanotubes is 30-50 nm.
5. The lip sheet formula for enhancing the wear resistance of the lip according to claim 1, characterized in that: The glass fiber has a diameter of 14-16 μm and a length of 120-150 μm.
6. The lip sheet formulation for enhancing the wear resistance of the lip according to claim 1, characterized in that: The particle size of the molybdenum disulfide is 120-180 μm.
7. The production process of a lip sheet formula for enhancing lip wear resistance according to claim 1, characterized in that: The following steps are involved: Step 1: refrigerate PTFE, glass fiber, molybdenum disulfide, talc and modified carbon nanotubes respectively, add them into a high-speed mixer according to weight parts, stir them evenly, and then dry, crush and sieve them in sequence to obtain crushed materials; Step 2: The crushed materials are pressed and sintered in stages in sequence to obtain the product.
8. The production process of a lip sheet formula for enhancing lip wear resistance according to claim 7, characterized in that: The refrigeration temperature is ≤-20°C and the refrigeration time is 24-36h.
9. The production process of a lip sheet formula for enhancing lip wear resistance according to claim 7, characterized in that: The process steps of the segmented sintering are as follows: Heating from room temperature to 180°C at a rate of 20-25°C / 10min; From 180℃ to 290℃, the heating rate is 10-15℃ / 10min; Heat from 290℃ to 330℃ at a rate of 3-5℃ / 10min, and keep at 330℃ for 90-100min; Heat from 330°C to 375°C at a rate of 3-5°C / 10min, and keep at 375°C for 180-200min.
Citation Information
Patent Citations
Preparing method of seal ring materials
CN106317720A
Self-adhesive carbon nanotube-polytetrafluoroethylene valve sealing ring
CN106398061A
Preparing method of dithiocarbamic acid-based functionalized carbon nano tube
CN106587012A
High-resilience, self-lubricating and wear-resistant polytetrafluoroethylene oil seal lip material and preparation method thereof
CN116082773A
Antifriction polymer composite material
RU2012146766A