Antibacterial sanitary product and preparation method thereof
The oxygen-containing groups of ABS plastic are increased by constant temperature treatment, and the use of chitosaccharide-modified carboxylic styrene butadiene and zinc oxide are used to solve the aging and compatibility problems of ABS plastic, improve its mechanical and antibacterial properties, and realize waste ABS efficient recycling.
Patent Information
- Application Number
- CN202410997756.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ABS plastic aging under the influence of environmental factors such as light, oxygen, and ultraviolet rays, resulting in a decrease in mechanical properties, and produce harmful gases during incineration, which pollutes the environment, and has poor compatibility with polymethyl methacrylate materials, resulting in blending properties. reduce.
The oxygen-containing active groups in waste ABS plastic are increased by constant temperature treatment, and the use of chitosaccharides and carboxy-styrene butadiene glue to chemically connect to enhance stability and antibacterial effect. Chitosaccharide-modified carboxy-styrene butadiene glue is used as a compatibility agent , reduce the interfacial tension between ABS and polymethyl methacrylate, improve compatibility and adhesion, and introduce zinc oxide to improve antibacterial properties.
It significantly improves the strength and toughness of waste ABS plastics, enhances compatibility with polymethyl methacrylate, improves mechanical properties, and significantly improves the antibacterial properties of bathroom products through the antibacterial mechanism of chitin oligosaccharide and zinc oxide. .
Smart Images

Figure BDA0004960734330000041 
Figure BDA0004960734330000051 
Figure BDA0004960734330000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sanitary ware products and relates to an antibacterial sanitary ware product and a preparation method thereof. Background Art
[0002] As an engineering plastic, ABS has a large output and is widely used. It is copolymerized by three monomers: acrylonitrile, butadiene, and styrene, so it has the performance characteristics of these three components. ABS plastic plays an important role in many fields such as home appliances, transportation, daily necessities, and office equipment, among which the application in the home appliance field accounts for as high as 63%. Looking to the future, the application fields of ABS materials will be further expanded.
[0003] Although the service life of ABS plastic can reach more than ten years, it will gradually age, turn yellow and become brittle under the influence of environmental factors such as light, oxygen and ultraviolet rays, resulting in a significant decrease in mechanical properties. If these waste plastics are not treated, it may take up to a hundred years for them to degrade naturally. However, if these waste plastics are directly incinerated, harmful gases will be produced, causing pollution to the ecological environment. Therefore, it is very important to explore the recycling methods of waste ABS. Understanding the aging mechanism of ABS plastics, improving its comprehensive performance, and enabling it to be put into use again can not only reduce the environmental burden, but also save non-renewable resources such as oil.
[0004] Polymethyl methacrylate is light, strong, resistant to aging, does not deform or discolor, and has a long service life. It has a high density, a smooth surface, no micropores, is easy to clean, and does not harbor dirt. It is widely used as a material for bathroom products.
[0005] However, ABS and polymethyl methacrylate have significant differences in solubility parameters and are therefore thermodynamically incompatible. Simply blending the two will result in severe phase separation, which will reduce the performance of the blend. Therefore, when using these two materials, their compatibility needs to be fully considered. Summary of the invention
[0006] The purpose of the present invention is to provide an antibacterial sanitary ware product and a preparation method thereof. The present invention uses constant temperature treatment of waste ABS plastics to increase oxygen-containing active groups, and uses chitosan oligosaccharides and carboxylated styrene butadiene rubber to connect through chemical bonds to enhance stability and antibacterial effects. Chitosan oligosaccharide-modified carboxylated styrene butadiene rubber and SBG are compounded as compatibilizers to reduce ABS interfacial tension, improve compatibility and adhesion, improve mechanical properties, increase zinc oxide dispersibility, and improve the antibacterial properties of sanitary ware products through the antibacterial mechanism of chitosan oligosaccharides and zinc oxide.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A method for preparing an antibacterial bathroom product, the method comprising the following steps:
[0009] S1, after the ABS particles are treated at a constant temperature, a compatibilizer is added and melted and extruded, and the particles are cut and dried to obtain particles; the compatibilizer is composed of SBG and chitosan oligosaccharide modified carboxylated styrene-butadiene rubber;
[0010] S2, stirring and mixing the filler and the silane coupling agent, then adding polymethyl methacrylate, the granules and the auxiliary materials, mixing, melt-extruding, and pelletizing to obtain prefabricated particles;
[0011] S3. The prefabricated particles are melted and injected into a mold, and then cooled, molded, ground and polished to obtain an antibacterial bathroom product.
[0012] As a preferred technical solution of the present invention, in step S1, the constant temperature treatment is 180-200°C for 2-2.5h; the temperature of the melt extrusion is 210-220°C; in step S2, the temperature of the melt extrusion is 230-240°C;
[0013] As a preferred technical solution of the present invention, the SBG is a styrene-butadiene-glycidyl methacrylate terpolymer with a molecular weight of 18,000.
[0014] As a preferred technical solution of the present invention, the ABS particles are selected from waste ABS plastics. The carbon-carbon double bonds (C=C) of the butadiene phase in the aged waste ABS plastics are broken to generate hydroperoxides, which continue to decompose to generate oxygen-containing groups such as carbonyl, carboxyl, and hydroxyl. Finally, phase separation occurs inside the plastic, the plastic becomes brittle and yellow, and the mechanical properties are significantly reduced. The present invention uses constant temperature treatment to allow the waste ABS plastics to generate more oxygen-containing groups such as carbonyl, carboxyl, and hydroxyl, so that the epoxy groups on the SBG react with the carboxyl, The hydroxyl groups are grafted, so that SBG can effectively reinforce the waste ABS and increase the bonding between the chitosan oligosaccharide-modified carboxylated styrene butadiene rubber and the waste ABS. Due to the amino, carboxyl and hydroxyl functional groups contained in the chitosan oligosaccharide-modified carboxylated styrene butadiene rubber, the waste ABS is further reinforced by interacting with the carbonyl, carboxyl, hydroxyl and other oxygen-containing groups of the waste ABS. The strength and toughness of the waste ABS are improved through the above-mentioned joint action, while the chitosan oligosaccharide containing antibacterial ingredients is introduced. The chitosan and carboxylated styrene butadiene rubber are connected by chemical bonds, which improves the stability of the chitosan oligosaccharide and significantly improves its antibacterial effect.
[0015] In addition, chitosan oligosaccharide-modified carboxylated styrene-butadiene rubber contains butadiene phase and styrene phase. Combined with the butadiene phase, styrene phase and glycidyl methacrylate phase on SBG, it can reduce the interfacial tension between waste ABS and polymethyl methacrylate, improve the compatibility and interfacial adhesion between the two, thereby improving the dispersibility of ABS in the polymethyl methacrylate system, significantly increasing the compatibility of waste ABS and polymethyl methacrylate, and thus improving the mechanical properties of sanitary products.
[0016] As a preferred technical solution of the present invention, the particles obtained by melt extrusion of waste ABS and a compatibilizer contain a large number of hydroxyl groups, carboxyl groups and amino groups, which interact with zinc oxide, increase its dispersibility in the system, and further improve the antibacterial properties of sanitary products through the different antibacterial mechanisms of chitosan oligosaccharides and zinc oxide.
[0017] As a preferred technical solution of the present invention, the compatibilizer is prepared by mixing SBG and chitosan oligosaccharide-modified carboxylated styrene-butadiene rubber in a mass ratio of 1.5:2-2.2.
[0018] As a preferred technical solution of the present invention, the filler is one or more of nano-aluminum hydroxide, zinc oxide, quartz powder and microsilica powder.
[0019] As a preferred technical solution of the present invention, the auxiliary material is prepared by mixing antioxidant 1076 and stearic acid in a mass ratio of 1:1.2-1.6.
[0020] As a preferred technical solution of the present invention, the silane coupling agent is one or more of KH-550 silane coupling agent, KH-560 silane coupling agent and KH-570 silane coupling agent.
[0021] As a preferred technical solution of the present invention, the preparation method of the chitosan oligosaccharide modified carboxylated styrene butadiene rubber comprises the following steps: chitosan oligosaccharide and acetic acid aqueous solution are stirred and mixed, ammonium cerium nitrate is added as an initiator under a nitrogen atmosphere, carboxylated styrene butadiene rubber latex is slowly added dropwise under stirring, heating and stirring after the addition is completed, filtering out the product, and freeze-drying to obtain chitosan oligosaccharide modified carboxylated styrene butadiene rubber.
[0022] As a preferred technical solution of the present invention, the heating and stirring is stirring at a temperature of 40-45° C. for 6-8 hours; the acetic acid aqueous solution is prepared by mixing acetic acid and deionized water in a volume ratio of 1:1.
[0023] As a preferred technical solution of the present invention, the mass ratio of the chitosan oligosaccharide, the acetic acid aqueous solution, the ammonium cerium nitrate and the carboxylated styrene butadiene latex is 1-1.2g:25-28mL:1.6-1.8g:3.5-4g; the solid content of the carboxylated styrene butadiene latex is 48-50%. Under the action of the ammonium cerium nitrate, the chitosan oligosaccharide will generate a large number of free radicals. Under the attack of the free radicals, the unsaturated carbon-carbon double bonds of the carboxylated styrene butadiene rubber are opened, chemical bonds are formed with the chitosan oligosaccharide molecules, and a grafting reaction occurs.
[0024] The present invention discloses an antibacterial sanitary ware product prepared by the above-mentioned preparation method, wherein the antibacterial sanitary ware product comprises the following components in parts by weight:
[0025]
[0026] Beneficial effects of the present invention:
[0027] The present invention generates more oxygen-containing groups in waste ABS plastics through constant temperature treatment, promotes the grafting of epoxy groups on SBG with waste ABS plastics, and at the same time, the epoxy groups on SBG can also be grafted with chitosan oligosaccharide-modified carboxylated styrene butadiene rubber, thereby enhancing the strength and toughness of waste ABS. At the same time, the amino, carboxyl and hydroxyl functional groups in the chitosan oligosaccharide-modified carboxylated styrene butadiene rubber interact with the oxygen-containing groups of waste ABS, further improving the reinforcement effect. In addition, chitosan oligosaccharide and carboxylated styrene butadiene rubber are connected by chemical bonds, thereby improving the stability of chitosan oligosaccharide and enhancing its antibacterial effect. The butadiene phase and styrene phase of the chitosan oligosaccharide-modified carboxylated styrene butadiene rubber are combined with the corresponding phases of SBG to reduce the interfacial tension between waste ABS and polymethyl methacrylate, improve the compatibility and interfacial adhesion, and improve the dispersibility of ABS in the polymethyl methacrylate system. The melt-extruded waste ABS and compatibilizer particles contain a large number of hydroxyl, carboxyl and amino groups, which interact with zinc oxide to increase its dispersibility in the system and improve the antibacterial properties of sanitary products through the antibacterial mechanism of chitosan oligosaccharides and zinc oxide. DETAILED DESCRIPTION
[0028] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0029] Example 1
[0030] The antibacterial sanitary ware product comprises the following components by weight:
[0031]
[0032] The auxiliary material is prepared by mixing antioxidant 1076 and stearic acid in a mass ratio of 1:1.2;
[0033] The compatibilizer is prepared by mixing SBG and chitosan oligosaccharide modified carboxyl styrene-butadiene rubber in a mass ratio of 1.5:2;
[0034] The filler is a mixture of nano-aluminum hydroxide, zinc oxide, quartz powder and microsilicon powder in a mass ratio of 3:2:1.5:1.8;
[0035] The preparation method of the chitosan oligosaccharide modified carboxylated styrene butadiene rubber comprises the following steps: after chitosan oligosaccharide and acetic acid aqueous solution are stirred and mixed, ammonium cerium nitrate is added as an initiator under a nitrogen atmosphere, carboxylated styrene butadiene rubber latex with a solid content of 48% is slowly dripped under stirring, after the dripping is completed, it is stirred at a temperature of 40°C for 8 hours, the product is filtered out, and after freeze-drying, the chitosan oligosaccharide modified carboxylated styrene butadiene rubber is obtained; wherein the acetic acid aqueous solution is prepared by mixing acetic acid and deionized water in a volume ratio of 1:1; the mass ratio of the chitosan oligosaccharide, the acetic acid aqueous solution, the ammonium cerium nitrate and the carboxylated styrene butadiene latex is 1g:25mL:1.6g:3.5g.
[0036] A method for preparing an antibacterial bathroom product, the method comprising the following steps:
[0037] S1. Keep ABS particles at a constant temperature of 180° C. for 2.5 hours, then add a compatibilizer and melt extrude at 210° C., cut into particles and then dry to obtain particles; the compatibilizer is composed of SBG and chitosan oligosaccharide modified carboxylated styrene-butadiene rubber;
[0038] S2, after the filler and KH-560 silane coupling agent are stirred and mixed, polymethyl methacrylate, particulate matter and auxiliary materials are added, mixed, melt-extruded at 230° C., and pelletized to obtain prefabricated particles;
[0039] S3. The prefabricated particles are melted and injected into a mold, and then cooled, molded, ground and polished to obtain an antibacterial bathroom product.
[0040] Example 2
[0041] The antibacterial sanitary ware product comprises the following components by weight:
[0042]
[0043] The auxiliary material is prepared by mixing antioxidant 1076 and stearic acid in a mass ratio of 1:1.4;
[0044] The compatibilizer is prepared by mixing SBG and chitosan oligosaccharide modified carboxyl styrene-butadiene rubber in a mass ratio of 1.5:2.1;
[0045] The filler is a mixture of nano-aluminum hydroxide, zinc oxide, quartz powder and microsilica powder in a mass ratio of 3:2:1.5:1.8;
[0046] The preparation method of chitosan oligosaccharide modified carboxylated styrene butadiene rubber comprises the following steps: chitosan oligosaccharide and acetic acid aqueous solution are stirred and mixed, ammonium cerium nitrate is added as an initiator under a nitrogen atmosphere, carboxylated styrene butadiene rubber latex with a solid content of 49% is slowly dripped under stirring, and after the dripping is completed, it is stirred at a temperature of 42° C. for 7 hours, the product is filtered out, and freeze-dried to obtain chitosan oligosaccharide modified carboxylated styrene butadiene rubber; wherein the acetic acid aqueous solution is prepared by mixing acetic acid and deionized water in a volume ratio of 1:1; the mass ratio of the chitosan oligosaccharide, the acetic acid aqueous solution, the ammonium cerium nitrate and the carboxylated styrene butadiene latex is 1.1 g:26 mL:1.7 g:3.8 g.
[0047] A method for preparing an antibacterial bathroom product, the method comprising the following steps:
[0048] S1. Keep ABS particles at a constant temperature of 190° C. for 2.2 hours, then add a compatibilizer and melt extrude at 215° C., cut into particles and then dry to obtain particles; the compatibilizer is composed of SBG and chitosan oligosaccharide modified carboxylated styrene-butadiene rubber;
[0049] S2, after the filler and KH-560 silane coupling agent are stirred and mixed, polymethyl methacrylate, particulate matter and auxiliary materials are added, mixed, melt-extruded at 235° C., and pelletized to obtain prefabricated particles;
[0050] S3. The prefabricated particles are melted and injected into a mold, and then cooled, molded, ground and polished to obtain an antibacterial bathroom product.
[0051] Example 3
[0052] The antibacterial sanitary ware product comprises the following components by weight:
[0053]
[0054] The auxiliary material is prepared by mixing antioxidant 1076 and stearic acid in a mass ratio of 1:1.6;
[0055] The compatibilizer is prepared by mixing SBG and chitosan oligosaccharide modified carboxyl styrene-butadiene rubber in a mass ratio of 1.5:2.2;
[0056] The filler is a mixture of nano-aluminum hydroxide, zinc oxide, quartz powder and microsilica powder in a mass ratio of 3:2:1.5:1.8;
[0057] The preparation method of the chitosan oligosaccharide modified carboxylated styrene butadiene rubber comprises the following steps: after chitosan oligosaccharide and acetic acid aqueous solution are stirred and mixed, ammonium cerium nitrate is added as an initiator under a nitrogen atmosphere, carboxylated styrene butadiene rubber latex with a solid content of 50% is slowly dripped under stirring, after the dripping is completed, it is stirred at a temperature of 45°C for 6 hours, the product is filtered out, and after freeze-drying, the chitosan oligosaccharide modified carboxylated styrene butadiene rubber is obtained; wherein the acetic acid aqueous solution is prepared by mixing acetic acid and deionized water in a volume ratio of 1:1; the mass ratio of the chitosan oligosaccharide, the acetic acid aqueous solution, the ammonium cerium nitrate and the carboxylated styrene butadiene latex is 1.2g:28mL:1.8g:4g.
[0058] A method for preparing an antibacterial bathroom product, the method comprising the following steps:
[0059] S1. Keep ABS particles at a constant temperature of 200°C for 2 hours, then add a compatibilizer and melt extrude at 220°C, cut into particles and then dry to obtain particles; the compatibilizer is composed of SBG and chitosan oligosaccharide modified carboxylated styrene-butadiene rubber;
[0060] S2, after the filler and KH-560 silane coupling agent are stirred and mixed, polymethyl methacrylate, particulate matter and auxiliary materials are added, mixed, melt-extruded at 240° C., and pelletized to obtain prefabricated particles;
[0061] S3. The prefabricated particles are melted and injected into a mold, and then cooled, molded, ground and polished to obtain an antibacterial bathroom product.
[0062] Comparative Example 1
[0063] Compared with Example 2, the difference in Comparative Example 1 is that carboxylated styrene butadiene latex replaces chitosan oligosaccharide-modified carboxylated styrene butadiene rubber, and the other components, preparation steps and parameters are the same.
[0064] Comparative Example 2
[0065] Compared with Example 2, the difference in Comparative Example 2 is that chitosan oligosaccharide replaces chitosan oligosaccharide-modified carboxylated styrene-butadiene rubber, and the other components, preparation steps and parameters are the same.
[0066] Comparative Example 3
[0067] Compared with Example 2, Comparative Example 3 is different in that:
[0068] The mixture is used to replace the chitosan oligosaccharide modified carboxyl styrene-butadiene rubber, and the preparation of the mixture comprises the following steps:
[0069] After chitosan oligosaccharide and acetic acid aqueous solution are stirred and mixed, carboxylated styrene butadiene latex with a solid content of 50% is slowly added dropwise under stirring in a nitrogen atmosphere. After the addition is completed, the mixture is stirred at 45°C for 6 hours and dried to obtain a mixture; wherein the acetic acid aqueous solution is prepared by mixing acetic acid and deionized water in a volume ratio of 1:1; and the mass ratio of the chitosan oligosaccharide, acetic acid aqueous solution and carboxylated styrene butadiene latex is 1.2g:28mL:4g.
[0070] The remaining components, preparation steps and parameters were the same.
[0071] Comparative Example 4
[0072] Compared with Example 2, the difference in Comparative Example 4 is that the compatibilizer is SBG, and the other components, preparation steps and parameters are the same.
[0073] Comparative Example 5
[0074] Compared with Example 2, the difference in Comparative Example 5 is that the compatibilizer is chitosan oligosaccharide modified carboxylated styrene-butadiene rubber, and the other components, preparation steps and parameters are the same.
[0075] Comparative Example 6
[0076] Compared with Example 2, the difference in Comparative Example 6 is that step S1 does not perform constant temperature treatment, and the remaining components, preparation steps and parameters are the same.
[0077] Comparative Example 7
[0078] Compared with Example 2, Comparative Example 7 is different in that:
[0079] A method for preparing an antibacterial bathroom product, the method comprising the following steps:
[0080] S1. Keeping ABS particles at a constant temperature of 190° C. for 2.2 h, obtaining particles;
[0081] S2, after the filler and KH-560 silane coupling agent are stirred and mixed, polymethyl methacrylate, particulate matter, auxiliary materials and compatibilizer are added, mixed, melt-extruded at 235° C., and pelletized to obtain prefabricated particles; the compatibilizer is composed of SBG and chitosan oligosaccharide modified carboxylated styrene-butadiene rubber;
[0082] S3. The prefabricated particles are melted and injected into a mold, and then cooled, molded, ground and polished to obtain an antibacterial bathroom product.
[0083] The remaining components, preparation steps and parameters were the same.
[0084] test:
[0085] The prefabricated particles obtained in Examples 1-3 and Comparative Examples 1-6 were tested as follows. The test results are shown in Table 1.
[0086] Tensile strength test: According to GB / T1040.2-2006; test speed is 50mm / min, test speed is 1.3mm / min;
[0087] Notched impact strength test: according to GB / T1043-2008;
[0088] Antibacterial performance test: prepare a sample with a diameter of 6mm and a height of 2mm, put it into a culture medium containing Staphylococcus aureus and Escherichia coli, maintain 37℃ / 24h, test the diameter of the antibacterial ring, and culture it for 5 consecutive times to take the average value. The larger the diameter of the antibacterial ring, the better the antibacterial performance.
[0089] Table 1
[0090] Tensile strength(MPa) <![CDATA[Notched impact strength (KJ / m 2 )]]> Antibacterial diameter (mm) Example 1 42.6 41.4 30 Example 2 42.8 41.7 31 Example 3 42.5 41.2 29 Comparative Example 1 36.2 35.0 21 Comparative Example 2 33.5 32.4 25 Comparative Example 3 37.0 35.8 26 Comparative Example 4 31.3 30.1 18 Comparative Example 5 30.1 28.8 22 Comparative Example 6 33.8 32.7 27 Comparative Example 7 36.0 34.8 26
[0091] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-7, the mechanical properties of tensile strength and notched impact strength of the sanitary ware products prepared in Examples 1-3 of the present invention are significantly better than those of Comparative Examples 1-7; at the same time, the antibacterial effect of the sanitary ware products prepared in the present invention is more excellent.
[0092] By comparing Examples 1-3 with Comparative Examples 1-7, combined with the analysis of Table 1, it can be seen that the use of constant temperature treatment of waste ABS plastics increases the oxygen-containing active groups, promotes the grafting with SBG and chitosan oligosaccharide modified carboxylated styrene butadiene rubber, and enhances its strength and toughness. The functional groups in chitosan oligosaccharides interact with waste ABS to improve the reinforcement effect. Chitosan oligosaccharides are connected to carboxylated styrene butadiene rubber through chemical bonds to enhance stability and antibacterial effects. The butadiene phase and styrene phase of the modified glue are combined with SBG to reduce interfacial tension, improve compatibility and adhesion, and improve the dispersibility of ABS in polymethyl methacrylate. The particles obtained by melting ABS and the compatibilizer interact with zinc oxide to increase dispersibility, and through the antibacterial mechanism of chitosan oligosaccharides and zinc oxide, the antibacterial properties of sanitary products are improved.
[0093] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing an antibacterial bathroom product, characterized in that: The preparation method comprises the following steps: S1, after the ABS particles are treated at a constant temperature, a compatibilizer is added and melted and extruded, and the particles are cut and dried to obtain particles; the compatibilizer is composed of SBG and chitosan oligosaccharide modified carboxylated styrene-butadiene rubber; S2, after the filler and the silane coupling agent are stirred and mixed, polymethyl methacrylate, the granules and the auxiliary materials are added, mixed, melt-extruded, and pelletized to obtain prefabricated particles; S3. The prefabricated particles are melted and injected into a mold, and then cooled, molded, ground and polished to obtain an antibacterial bathroom product.
2. The method for preparing an antibacterial sanitary ware product according to claim 1, characterized in that: In step S1, the constant temperature treatment is performed at 180-200°C for 2-2.5 hours; the temperature of the melt extrusion is 210-220°C; and in step S2, the temperature of the melt extrusion is 230-240°C.
3. The method for preparing an antibacterial sanitary ware product according to claim 1, characterized in that: The compatibilizer is prepared by mixing SBG and chitosan oligosaccharide modified carboxyl styrene-butadiene rubber in a mass ratio of 1.5:2-2.
2.
4. The method for preparing an antibacterial sanitary ware product according to claim 1, characterized in that: The filler is one or more of nano-aluminum hydroxide, zinc oxide, quartz powder and microsilica powder.
5. The method for preparing an antibacterial sanitary ware product according to claim 1, characterized in that: The auxiliary material is prepared by mixing antioxidant 1076 and stearic acid in a mass ratio of 1:1.2-1.
6.
6. The method for preparing an antibacterial sanitary ware product according to claim 1, characterized in that: The silane coupling agent is one or more of KH-550 silane coupling agent, KH-560 silane coupling agent and KH-570 silane coupling agent.
7. The method for preparing an antibacterial sanitary ware product according to claim 3, characterized in that: The preparation method of chitosan oligosaccharide modified carboxylated styrene butadiene rubber comprises the following steps: chitosan oligosaccharide and acetic acid aqueous solution are stirred and mixed, ammonium cerium nitrate is added as an initiator under a nitrogen atmosphere, carboxylated styrene butadiene rubber latex is slowly added dropwise under stirring, heating and stirring after the addition is completed, filtering out the product, and freeze-drying to obtain chitosan oligosaccharide modified carboxylated styrene butadiene rubber.
8. The method for preparing an antibacterial sanitary ware product according to claim 7, characterized in that: The heating and stirring is stirring at a temperature of 40-45° C. for 6-8 hours; the acetic acid aqueous solution is prepared by mixing acetic acid and deionized water in a volume ratio of 1:
1.
9. The method for preparing an antibacterial sanitary ware product according to claim 7, characterized in that: The mass ratio of the chitosan oligosaccharide, the acetic acid aqueous solution, the cerium ammonium nitrate and the carboxylated styrene butadiene latex is 1-1.2 g: 25-28 mL: 1.6-1.8 g: 3.5-4 g; and the solid content of the carboxylated styrene butadiene latex is 48-50%.
10. An antibacterial sanitary ware product prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The antibacterial sanitary ware product comprises the following components by weight: Polymethyl methacrylate 70-80 parts ABS particles 26-30 parts Compatibilizer 8-10 parts 12-15 servings of filling Silane coupling agent 1-1.5 parts 1.0-2.5 parts of auxiliary materials.
Citation Information
Patent Citations
Chitosan oligosaccharide grafted copolymer G1.0 as well as preparation method and application thereof
CN108192000A
High-strength wear-resistant PET material and preparation method thereof
CN118256071A
High-gloss scratch-resistant ABS / PMMA (acrylonitrile butadiene styrene / polymethyl methacrylate) alloy material and preparation method thereof
CN118344699A