Resin-based composite material and preparation method thereof

By adding glass microbeads and nano-toughening particles to the resin-based composite material, adjusting the formula, combining epoxy resin and other materials, the problem of insufficient density and performance of carbon fiber reinforced resin-based composite material is solved, and lightweight and high performance is achieved The preparation of resin-based composite materials is suitable for high-end applications.

CN118909401APending Publication Date: 2024-11-08ZHONGFU SHENYING CARBON FIBER
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411125155.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing carbon fiber reinforced resin-based composites have insufficient density and performance in certain areas where high performance needs are required, making it difficult to meet the requirements of special applications.

Method used

By adding glass beads and nano-toughening particles to the resin-based composite material and adjusting their proportions, combining epoxy resin prepolymer mixture, ethylene-octene copolymer and curing agent, and using a specific mixing and curing process, prepare Lightweight, high-performance composite materials.

Benefits of technology

It effectively improves the mechanical properties of composite materials and reduces their density, and is suitable for high-end applications such as aerospace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909401A_ABST
    Figure CN118909401A_ABST
Patent Text Reader

Abstract

The invention discloses a resin-based composite material and a preparation method thereof, and relates to the technical field of composite materials. The resin-based composite material comprises the following raw materials in parts by weight: 30-55 parts of a resin matrix; 45-70 parts by weight of reinforcing fibers; 1.2 to 15.0 parts by weight of glass beads; and 1.2-8.8 parts by weight of a curing agent. According to the resin-based composite material disclosed by the invention, the reinforcing fibers and the glass beads are used as reinforcing materials, so that the density of the composite material can be reduced while the mechanical property of the composite material is effectively improved, and the light and high-performance composite material is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a resin-based composite material and a preparation method thereof. Background Art

[0002] Composite materials refer to materials composed of two or more components, and many of their properties are usually superior to those of single-component materials. Among them, fiber-reinforced resin-based composite materials are composite materials with fiber as reinforcing agent and resin as matrix material. They have the advantages of high specific strength, high specific modulus, good fatigue resistance and excellent corrosion resistance, and have become the preferred material in many high-end application fields.

[0003] At present, the density of carbon fiber reinforced resin matrix composite materials is about 1.7g / cm 3 This low density, combined with its high specific strength and high specific modulus, makes carbon fiber reinforced resin-based composites widely used in aerospace, sports equipment, automotive technology and other fields. However, in some special fields, higher requirements are placed on the density and high performance of carbon fiber reinforced resin-based composites. Summary of the invention

[0004] In order to solve the above technical problems, the present application aims to provide a resin-based composite material and a preparation method thereof, wherein the resin-based composite material has the advantages of light weight and high mechanical properties.

[0005] According to a first aspect of the present application, a resin-based composite material is provided, comprising the following raw materials in parts by weight:

[0006] 30-55 parts by weight of resin matrix;

[0007] Reinforcement fiber 45-70 parts by weight;

[0008] Glass microspheres 1.2-15.0 parts by weight;

[0009] Curing agent 1.2-7.7 parts by weight.

[0010] In some embodiments of the present application, the weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0011] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix.

[0012] In some embodiments of the present application, the glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0013] In some embodiments of the present application, the resin matrix includes the following raw materials in parts by weight:

[0014] 40-50 parts by weight of epoxy resin prepolymer mixture;

[0015] 15-30 parts by weight of ethylene-octene copolymer;

[0016] 10-20 parts by weight of nano toughening particles.

[0017] In some embodiments of the present application, the epoxy resin prepolymer mixture includes a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin.

[0018] In some embodiments of the present application, when the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of the bisphenol A epoxy resin, the bisphenol F epoxy resin and the hydantoin epoxy resin is 2-4:1-3:1.

[0019] In some embodiments of the present application, the weight ratio of the sum of the ethylene-octene copolymer and the nano-toughening particles to the epoxy resin prepolymer mixture is 0.65-0.85:1.

[0020] According to a second aspect of the present application, a method for preparing a composite material is provided. The method for preparing a composite material is used to prepare the resin-based composite material as described above. The method comprises:

[0021] Mixing the resin matrix and the glass microbeads at a first preset temperature to obtain a first mixture;

[0022] mixing the first mixture with the curing agent at a second preset temperature to obtain a second mixture;

[0023] impregnating the reinforcing fiber with the second mixture to obtain a prepreg;

[0024] The prepreg is cured under a preset curing system to obtain the resin-based composite material.

[0025] In some embodiments of the present application, before mixing the resin matrix and the glass microspheres at the first preset temperature, the preparation method further comprises:

[0026] The initial glass microspheres are immersed in an organic solvent and then dried to obtain the glass microspheres.

[0027] In some embodiments of the present application, the method for preparing the resin matrix includes:

[0028] The epoxy resin prepolymer mixture, the ethylene-octene copolymer and the nano toughening particles are mixed at a third preset temperature to obtain the resin matrix.

[0029] The technical solution provided by this application may have the following beneficial effects:

[0030] The resin-based composite material of the present application uses reinforcing fibers and glass microspheres as reinforcing materials, which can effectively improve the mechanical properties of the composite material while reducing the density of the composite material, thereby obtaining a lightweight, high-performance composite material.

[0031] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0033] Figure 1 The present invention is a flow chart of a method for preparing a composite material according to an exemplary embodiment. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme of the present application will be clearly and completely described below in combination with the embodiments of the present application and the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be arbitrarily combined with each other.

[0035] The present application provides a resin-based composite material, comprising the following raw materials in parts by weight: 30-55 parts by weight of a resin matrix; 45-70 parts by weight of reinforcing fibers; 1.2-15.0 parts by weight of glass microspheres; and 1.2-7.7 parts by weight of a curing agent. By using reinforcing fibers and glass microspheres as reinforcing materials, the mechanical properties of the composite material can be effectively improved while reducing the density of the composite material, thereby obtaining a lightweight, high-performance composite material.

[0036] Some specific implementation modes described below are intended to facilitate those skilled in the art to understand the present embodiment, and the present embodiment is not limited to some specific implementation modes described below.

[0037] An exemplary embodiment of the present application provides a resin-based composite material, including the following raw materials in parts by weight:

[0038] 30-55 parts by weight of resin matrix;

[0039] Reinforcement fiber 45-70 parts by weight;

[0040] Glass microspheres 1.2-15.0 parts by weight;

[0041] Curing agent 1.2-7.7 parts by weight.

[0042] The resin matrix refers to a thermoplastic resin or a thermosetting resin as the matrix material, which can be used as an adhesive in a composite material to bond reinforcing materials such as reinforcing fibers and glass beads together to form a composite material with stable performance.

[0043] The reinforcing fiber is a fiber material with a reinforcing effect, which can improve the tensile strength and rigidity of the composite material. For example, the reinforcing fiber can be carbon fiber, glass fiber, aramid fiber, etc. For example, the reinforcing fiber in this embodiment can be selected from carbon fiber, model T800, and linear density 450g / km.

[0044] Glass beads are tiny spherical glass particles, usually made of borosilicate glass. They have a hollow structure and therefore have a low density. As fillers in composite materials, they can reduce the density of composite materials. In addition, the addition of glass beads can not only improve the mechanical properties of the composite materials, such as compressive strength and impact resistance, but also improve the fluidity of the liquid resin to improve the processing properties of the composite materials. Among them, the glass beads in this embodiment are composited with polyolefin as the carrier by a melt blending process, and their density is 0.65g / cm 3 The obtained glass microspheres have good compatibility with the resin matrix and can further improve the mechanical properties of the composite material.

[0045] In addition, glass microspheres, as a spherical filler, can provide better isotropy, while reinforcing fibers enhance the anisotropy of the material. By compounding the two, these two properties can be balanced. Moreover, glass microspheres can also be filled into the gaps between reinforcing fibers to improve filling efficiency, reduce the amount of resin used, improve the overall performance of the composite material, and reduce costs.

[0046] The curing agent can initiate and accelerate the curing reaction of the resin matrix, and improve the hardness, strength, toughness and other properties of the composite material. Exemplarily, the curing agent can be an amine curing agent, an anhydride curing agent, an isocyanate curing agent, etc. For example, the curing agent in this embodiment can be triethylenetetramine.

[0047] In this embodiment, the resin matrix, reinforcing fibers, glass beads and curing agent are compounded according to the above-mentioned specific proportions, so that the composite material obtained has the advantages of light weight and good mechanical properties, and is suitable for application in high-end fields such as aerospace.

[0048] For example, in one embodiment, a resin-based composite material includes the following raw materials in parts by weight:

[0049] 30 parts by weight of resin matrix;

[0050] 45 parts by weight of reinforcing fiber;

[0051] 1.2 parts by weight of glass microspheres;

[0052] 1.2 parts by weight of curing agent.

[0053] In another embodiment, a resin-based composite material includes the following raw materials in parts by weight:

[0054] 45 parts by weight of resin matrix;

[0055] 60 parts by weight of reinforcing fiber;

[0056] 7.5 parts by weight of glass microspheres;

[0057] 5.5 parts by weight of curing agent.

[0058] In another embodiment, a resin-based composite material includes the following raw materials in parts by weight:

[0059] Resin matrix 55 parts by weight;

[0060] 70 parts by weight of reinforcing fiber;

[0061] Glass microspheres 15.0 parts by weight;

[0062] Curing agent 7.7 parts by weight.

[0063] In an exemplary embodiment, the weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0064] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix.

[0065] In this embodiment, the comprehensive performance of the composite material is improved by adjusting the ratio of glass microspheres to the resin matrix, and the ratio of the curing agent to the resin matrix.

[0066] Exemplarily, the weight of the glass microspheres is 15.8%, 18.4% or 23.4% of the weight of the resin matrix; the weight of the curing agent is 8.0%, 10.0% or 12.0% of the weight of the resin matrix.

[0067] In an exemplary embodiment, the glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0068] In this embodiment, the first glass microbeads and the second glass microbeads with two different particle sizes are compounded and used. The second glass microbeads with a particle size of 80-120 μm can be filled into the gaps of the reinforcing fibers and cooperate with the reinforcing fibers to form a supporting skeleton. The second glass microbeads with a particle size of 40-60 μm can be filled into the gaps of the first glass microbeads to improve the filling efficiency, reduce the amount of resin, improve the comprehensive performance of the composite material, and reduce the cost. Exemplarily, the weight ratio of the first glass microbeads to the second glass microbeads is 6:2, 6:2.5 or 6:3.

[0069] In an exemplary embodiment, the resin matrix includes the following raw materials in parts by weight:

[0070] 40-50 parts by weight of epoxy resin prepolymer mixture;

[0071] 15-30 parts by weight of ethylene-octene copolymer;

[0072] 10-20 parts by weight of nano toughening particles.

[0073] The epoxy resin prepolymer mixture includes a combination of various epoxy resins. As a thermosetting resin, epoxy resin has excellent bonding properties, mechanical properties, chemical corrosion resistance and other properties.

[0074] Ethylene-octene copolymer is a thermoplastic elastomer generated by copolymerization of ethylene monomer and octene monomer, which has good elasticity and can improve the toughness of the resin matrix. Ethylene-octene copolymer can be, for example, 8780 of Exxon Chemical, 8605L of SK of South Korea, 8180 of Dow Chemical, etc., or thermoplastic amino-modified ethylene-octene copolymer can be used.

[0075] The nano toughening particles are toughening materials with a nanometer particle size, for example, nano calcium carbonate, nano silicon dioxide, nano montmorillonite, nano alumina, nano fiber, etc., and the particle size thereof may be 10-200 nm.

[0076] In this embodiment, the resin matrix composed of the epoxy resin prepolymer mixture, the ethylene-octene copolymer and the nano toughening particles has excellent mechanical strength and toughness, and has better comprehensive performance.

[0077] Exemplarily, in one embodiment, the resin matrix includes the following raw materials in parts by weight:

[0078] 40 parts by weight of epoxy resin prepolymer mixture;

[0079] 15 parts by weight of ethylene-octene copolymer;

[0080] 10 parts by weight of nano toughening particles.

[0081] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0082] 42 parts by weight of epoxy resin prepolymer mixture;

[0083] 16.5 parts by weight of ethylene-octene copolymer;

[0084] 11 parts by weight of nano toughening particles.

[0085] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0086] 44 parts by weight of epoxy resin prepolymer mixture;

[0087] 18 parts by weight of ethylene-octene copolymer;

[0088] 14 parts by weight of nano toughening particles.

[0089] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0090] 45 parts by weight of epoxy resin prepolymer mixture;

[0091] 20 parts by weight of ethylene-octene copolymer;

[0092] 15 parts by weight of nano toughening particles.

[0093] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0094] 50 parts by weight of epoxy resin prepolymer mixture;

[0095] 20.5 parts by weight of ethylene-octene copolymer;

[0096] 19 parts by weight of nano toughening particles.

[0097] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0098] 46 parts by weight of epoxy resin prepolymer mixture;

[0099] 22 parts by weight of ethylene-octene copolymer;

[0100] 17 parts by weight of nano toughening particles.

[0101] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0102] 48 parts by weight of epoxy resin prepolymer mixture;

[0103] 25 parts by weight of ethylene-octene copolymer;

[0104] 18 parts by weight of nano toughening particles.

[0105] In another embodiment, the resin matrix includes the following raw materials in parts by weight:

[0106] 50 parts by weight of epoxy resin prepolymer mixture;

[0107] 30 parts by weight of ethylene-octene copolymer;

[0108] 20 parts by weight of nano toughening particles.

[0109] In an exemplary embodiment, the epoxy resin includes bisphenol A epoxy resin, bisphenol F epoxy resin, hydantoin epoxy resin, etc. Exemplarily, the epoxy resin prepolymer mixture includes a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin.

[0110] As a commonly used epoxy resin, bisphenol A epoxy resin has excellent strength and bonding properties, but its heat resistance and toughness are slightly lower, and its weather resistance is poor. Compared with bisphenol A epoxy resin, bisphenol F epoxy resin has a smaller viscosity and has a good impregnation effect on reinforcing fibers, but its heat resistance is slightly lower. Hydantoin epoxy resin has low viscosity and good processing properties, and has good heat resistance and weather resistance. In the present embodiment, the epoxy resin prepolymer mixture formed by the compounding of the above-mentioned several epoxy resins has good comprehensive properties.

[0111] In an exemplary embodiment, when the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin is 2-4:1-3:1.

[0112] Illustratively, the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin is 2:1:1, 3:2:1 or 4:3:1.

[0113] In an exemplary embodiment, the weight ratio of the sum of the ethylene-octene copolymer, the nano toughening particles, and the epoxy resin prepolymer mixture is 0.65-0.85:1.

[0114] In this embodiment, the toughness of the composite material can be improved by compounding the ethylene-octene copolymer and the nano toughening particles. For example, the weight ratio of the sum of the ethylene-octene copolymer and the nano toughening particles to the epoxy resin prepolymer mixture is 0.65:1, 0.75:1 or 0.85:1.

[0115] like Figure 1As shown, an exemplary embodiment of the present application provides a method for preparing a composite material, the method for preparing a composite material is used to prepare the above resin-based composite material, and the preparation method includes:

[0116] S110, mixing the resin matrix and the glass microbeads at a first preset temperature to obtain a first mixture.

[0117] In step S110, the resin matrix and the glass microspheres may be mixed at a first preset temperature by melt blending, wherein the first preset temperature may be, for example, 140-160° C. Exemplarily, the resin matrix is ​​added to a planetary disperser and heated to 150° C. to melt the resin matrix to form a transparent homogeneous system; then, the glass microspheres are added to the system to obtain a first mixture.

[0118] S120, mixing the first mixture with the curing agent at a second preset temperature to obtain a second mixture.

[0119] In step S120, the first mixture is cooled and then mixed with a curing agent to avoid premature curing of the first mixture. The second preset temperature may be 50-60°C. At this temperature, the uniformity of the mixing of the first mixture and the curing agent can be improved while avoiding premature curing of the first mixture to obtain a second mixture with fluidity.

[0120] S130, impregnating the second mixture into reinforcing fibers to obtain a prepreg.

[0121] In step S130, a hot melt method may be used to impregnate the second mixture into the reinforcing fibers to obtain a prepreg.

[0122] S140, curing the prepreg under a preset curing system to obtain a resin-based composite material.

[0123] In step S140, the prepreg can be cured by heating the mold. The preset curing system can be a one-stage curing, for example, the curing temperature is 150°C and the curing time is 2 hours; it can also be a multi-stage curing, for example, a two-stage curing, first keeping it at a temperature of 100°C for 1 hour, and then keeping it at a temperature of 150°C for 2 hours.

[0124] For example, after cleaning the mold surface, apply a release agent on the mold surface; then place the prepreg in the mold, and after the mold is installed, pressurize the mold by lifting the hot press platform on the hot press plate, and perform temperature and pressure curing in a two-stage curing system. After the curing is completed, the temperature is lowered to 60°C at a rate of 0.8°C / min, the hot press is lowered, and the mold is opened to obtain a laminate of a resin-based composite material.

[0125] In an exemplary embodiment, before mixing the resin matrix and the glass microspheres at the first preset temperature, the preparation method further comprises:

[0126] The initial glass microbeads are immersed in an organic solvent and then dried to obtain glass microbeads.

[0127] In this embodiment, the organic solvent may be, for example, acetone. After the initial glass beads are soaked in acetone, impurities such as grease and dirt on the surface of the initial glass fiber can be removed to avoid the influence of impurities on the surface of the glass beads on the interface bonding strength between the glass beads and the resin matrix. The glass beads thus obtained can have a good reinforcement effect on the composite material.

[0128] In an exemplary embodiment, a method for preparing a resin matrix includes:

[0129] The epoxy resin prepolymer mixture, the ethylene-octene copolymer and the nano toughening particles are mixed at a third preset temperature to obtain a resin matrix.

[0130] In this embodiment, the epoxy resin prepolymer mixture, the ethylene-octene copolymer and the nano toughening particles are premixed to improve the uniformity of the mixing of the raw materials. The third preset temperature may be 140-160°C.

[0131] The specific implementation methods of the present application are further described below in conjunction with preferred embodiments, and examples of preferred value ranges of each component in the resin-based composite material provided in the present application are explained in detail.

[0132] Preferred Example 1

[0133] A resin-based composite material comprises the following raw materials in parts by weight:

[0134] 30-55 parts by weight of resin matrix;

[0135] Reinforcement fiber 45-70 parts by weight;

[0136] Glass microspheres 1.2-15.0 parts by weight;

[0137] 1.2-7.7 parts by weight of curing agent;

[0138] The weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0139] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix;

[0140] The glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0141] Preferred Example 2

[0142] A resin-based composite material comprises the following raw materials in parts by weight:

[0143] 30-55 parts by weight of resin matrix;

[0144] Reinforcement fiber 45-70 parts by weight;

[0145] Glass microspheres 1.2-15.0 parts by weight;

[0146] 1.2-7.7 parts by weight of curing agent;

[0147] The resin matrix includes the following raw materials in parts by weight:

[0148] 40-50 parts by weight of epoxy resin prepolymer mixture;

[0149] 15-30 parts by weight of ethylene-octene copolymer;

[0150] 10-20 parts by weight of nano toughening particles;

[0151] The weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0152] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix;

[0153] The glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0154] Preferred Example 3

[0155] A resin-based composite material comprises the following raw materials in parts by weight:

[0156] 30-55 parts by weight of resin matrix;

[0157] Reinforcement fiber 45-70 parts by weight;

[0158] Glass microspheres 1.2-15.0 parts by weight;

[0159] 1.2-7.7 parts by weight of curing agent;

[0160] The resin matrix includes the following raw materials in parts by weight:

[0161] 40-50 parts by weight of epoxy resin prepolymer mixture;

[0162] 15-30 parts by weight of ethylene-octene copolymer;

[0163] 10-20 parts by weight of nano toughening particles;

[0164] When the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin is 2-4:1-3:1;

[0165] The weight ratio of the sum of the ethylene-octene copolymer and the nano toughening particles to the epoxy resin prepolymer mixture is 0.65-0.85:1;

[0166] The weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0167] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix;

[0168] The glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0169] Preferred Example 4

[0170] A resin-based composite material comprises the following raw materials in parts by weight:

[0171] 40-46 parts by weight of resin matrix;

[0172] 60-66 parts by weight of reinforcing fiber;

[0173] Glass microspheres 6.3-10.8 parts by weight;

[0174] 3.6-5.5 parts by weight of curing agent;

[0175] The resin matrix includes the following raw materials in parts by weight:

[0176] 42-44 parts by weight of epoxy resin prepolymer mixture;

[0177] 16.5-18 parts by weight of ethylene-octene copolymer;

[0178] 11-14 parts by weight of nano toughening particles;

[0179] When the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin is 2.5-3:1.5-2:1;

[0180] The weight ratio of the sum of the ethylene-octene copolymer and the nano toughening particles to the epoxy resin prepolymer mixture is 0.65-0.77:1;

[0181] The weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0182] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix;

[0183] The glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0184] Preferred Example 5

[0185] A resin-based composite material comprises the following raw materials in parts by weight:

[0186] 40-46 parts by weight of resin matrix;

[0187] 60-66 parts by weight of reinforcing fiber;

[0188] Glass microspheres 6.3-10.8 parts by weight;

[0189] 3.6-5.5 parts by weight of curing agent;

[0190] The resin matrix includes the following raw materials in parts by weight:

[0191] 46-50 parts by weight of epoxy resin prepolymer mixture;

[0192] Ethylene-octene copolymer 20.5-22 parts by weight;

[0193] 17-19 parts by weight of nano toughening particles;

[0194] When the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin is 2.5-3.5:1.5-2.5:1;

[0195] The weight ratio of the sum of the ethylene-octene copolymer and the nano toughening particles to the epoxy resin prepolymer mixture is 0.79-0.85:1;

[0196] The weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix;

[0197] The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix;

[0198] The glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

[0199] Preferred Example 6

[0200] A resin-based composite material comprises the following raw materials in parts by weight:

[0201] 40-46 parts by weight of resin matrix;

[0202] 60-66 parts by weight of reinforcing fiber;

[0203] Glass microspheres 6.3-10.8 parts by weight;

[0204] 3.6-5.5 parts by weight of curing agent;

[0205] The resin matrix includes the following raw materials in parts by weight:

[0206] 46-50 parts by weight of epoxy resin prepolymer mixture;

[0207] Ethylene-octene copolymer 20.5-22 parts by weight;

[0208] 17-19 parts by weight of nano toughening particles;

[0209] When the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin is 2.5-3.5:1.5-2.5:1;

[0210] The weight ratio of the sum of the ethylene-octene copolymer and the nano toughening particles to the epoxy resin prepolymer mixture is 0.79-0.85:1;

[0211] The weight of the glass microspheres is 15.8-20.0% of the weight of the resin matrix;

[0212] The weight of the curing agent is 9.0-10.0% of the weight of the resin matrix;

[0213] The glass micro beads include first glass micro beads with a particle size of 40-60 μm and second glass micro beads with a particle size of 80-120 μm, and the weight ratio of the first glass micro beads to the second glass micro beads is 6:2-2.5.

[0214] In order to more clearly explain the technical solution of the present application, the present application lists specific embodiments of the resin-based composite material, and the beneficial effects of selecting the above-mentioned range of the content of each component will be explained by giving specific experimental data through specific embodiments.

[0215] Preparation example of resin matrix

[0216] Preparation Example 1: The resin matrix is ​​prepared by the following method:

[0217] Bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin are uniformly mixed in a weight ratio of 2:1:1 to obtain an epoxy resin prepolymer mixture; 40 kg of the epoxy resin prepolymer mixture, 15 kg of ethylene-octene copolymer and 10 kg of nano-calcium carbonate are uniformly mixed at a temperature of 150° C. to obtain a resin matrix.

[0218] In order to more clearly explain the technical solution of the present application, the present application also lists Preparation Examples 2-8 of the resin matrix, wherein the formulas of Preparation Examples 2-8 are shown in Table 1.

[0219] Table 1 shows a specific example of the resin matrix in the present application. It should be noted that, except for the parameters listed in Table 1, the other parameters of Preparation Examples 2-8 are substantially the same as those of Preparation Example 1.

[0220] Wherein, the C1 value in Table 1 is the weight ratio of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin in the epoxy resin prepolymer mixture;

[0221] The C2 value is the weight ratio of the sum of the ethylene-octene copolymer and the nano-toughening particles in the resin matrix to the epoxy resin prepolymer mixture.

[0222] Table 1 Raw material dosage of resin matrix in preparation examples 1-8

[0223]

[0224] Example

[0225] It should be noted that, unless otherwise specified, the raw materials in the following examples can be obtained from the market. Among them, the nano toughening particles are nano calcium carbonate; the curing agent is triethylenetetramine; and the reinforcing fiber is T800 carbon fiber.

[0226] Embodiment 1: A method for preparing a resin-based composite material, comprising the following steps:

[0227] (1) The initial glass microbeads are washed and soaked in an acetone solvent and then dried to obtain glass microbeads.

[0228] (2) 40 kg of the resin matrix and 8.0 kg of the glass microspheres were mixed uniformly at 150° C. to obtain a first mixture.

[0229] (3) After cooling the first mixture to 60° C., 3.6 kg of curing agent was added and mixed evenly to obtain a second mixture.

[0230] (4) The second mixture was impregnated with 60 kg of carbon fiber to obtain a prepreg.

[0231] (5) The prepreg is placed in a mold, first kept at a temperature of 100°C for 1 hour, and then kept at a temperature of 150°C for 2 hours. After curing, a resin-based composite material is obtained.

[0232] The glass microbeads are composed of first glass microbeads with an average particle size of 50 μm and second glass microbeads with an average particle size of 100 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2. The resin matrix is ​​prepared according to Preparation Example 3.

[0233] In order to more clearly explain the technical solution of the present application, the present application also lists Examples 2-16 of the resin-based composite material, wherein the formulas of Examples 2-16 are shown in Table 2.

[0234] Table 2 shows a specific embodiment of the resin-based composite material in the present application. It should be noted that, except for the parameters listed in Table 2, other parameters of Examples 2-16 and Example 1 are substantially the same.

[0235] Among them, the C3 value in Table 2 is the weight percentage of glass beads in the resin matrix;

[0236] The C4 value is the weight percentage of the curing agent in the resin matrix;

[0237] C5 value is the weight ratio of the first glass microbead to the second glass microbead;

[0238] Table 2 Raw material usage of the composite materials of Examples 1-16

[0239]

[0240] Table 2 (Continued) Raw material usage of the composite materials of Examples 1-16

[0241]

[0242] Comparative Example

[0243] Comparative Example 1: The main difference between this comparative example and Example 1 is that step (1) is not included, that is, the glass beads are not soaked and cleaned in acetone solvent.

[0244] Comparative Example 2: The main difference between this comparative example and Example 1 is that the amount of resin matrix used is 70 kg and the amount of carbon fiber used is 30 kg.

[0245] Comparative Example 3: The main difference between this comparative example and Example 1 is that the amount of resin matrix used is 25 kg and the amount of carbon fiber used is 75 kg.

[0246] Comparative Example 4: The main difference between this comparative example and Example 1 is that the weight ratio of the first glass microbeads to the second glass microbeads (ie, C5 value) is 6:1.

[0247] Comparative Example 5: The main difference between this comparative example and Example 1 is that the weight ratio of the first glass microbeads to the second glass microbeads (ie, C5 value) is 6:4.

[0248] Performance Testing

[0249] The carbon fiber composite laminates prepared in the examples and comparative examples were prepared into specimens for tensile and compression tests by engraving equipment. After being adjusted in a standard environment, the tensile strength, compressive strength and density performance tests were performed according to ASTM D 3039 and ASTM D 6641. The test results are recorded in Table 3.

[0250] Table 3 Performance test table of the composite materials of the embodiments and comparative examples

[0251] Tensile strength, MPa Compression strength, GPa <![CDATA[Density, g / cm 3 > Example 1 3000 1500 1.20 Example 2 2994 1495 1.24 Example 3 3004 1503 1.25 Example 4 3100 1540 1.51 Example 5 2445 1103 1.22 Example 6 2480 1190 1.21 Example 7 2632 1304 1.20 Example 8 2810 1410 1.20 Example 9 2940 1480 1.20 Example 10 2808 1440 1.21 Embodiment 11 2500 1200 1.23 Example 12 2100 1054 1.04 Example 13 3150 1560 1.20 Embodiment 14 3045 1524 1.20 Embodiment 15 2928 1433 1.20 Example 16 2807 1380 1.21 Comparative Example 1 2781 1320 1.24 Comparative Example 2 2450 1241 1.02 Comparative Example 3 2430 1182 1.62 Comparative Example 4 2731 1320 1.21 Comparative Example 5 2765 1340 1.25

[0252] It can be seen from the data in Table 1 and Table 2 that the composite material prepared by the method of the embodiment of the present application, the laminate thereof can have high tensile strength and compressive strength while maintaining a low density. It can be seen from Example 1 and Comparative Example 1 that the performance of the composite material can be improved after the glass beads are treated with acetone solvent. It can be seen from Example 1, Comparative Example 2 and Comparative Example 3 that a ratio of the resin matrix to the carbon fiber is too high or too low, which will lead to a decrease in the mechanical properties of the composite material. It can be seen from Example 1, Comparative Example 4 and Comparative Example 5 that a ratio between the first glass beads and the second glass beads is too high or too low, which will lead to a decrease in the mechanical properties of the composite material. It can be seen from Example 1 and Examples 5-12 that a weight percentage of the glass beads in the resin matrix and a weight percentage of the curing agent in the resin matrix are too high or too low, which will lead to a decrease in the mechanical properties of the composite material.

[0253] In summary, by adjusting the amount and ratio of each raw material in the composite material, the mechanical properties of the composite material can be improved so that it can maintain a higher mechanical strength while maintaining a lower density.

[0254] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0255] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application is described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A resin-based composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 30-55 parts by weight of resin matrix; 45-70 parts by weight of reinforcing fiber; Glass microspheres 1.2-15.0 parts by weight; Curing agent 1.2-7.7 parts by weight.

2. The resin-based composite material according to claim 1, characterized in that: The weight of the glass microspheres is 15.8-23.4% of the weight of the resin matrix; The weight of the curing agent is 8.0-12.0% of the weight of the resin matrix.

3. The resin-based composite material according to claim 1, characterized in that: The glass microbeads include first glass microbeads with a particle size of 40-60 μm and second glass microbeads with a particle size of 80-120 μm, and the weight ratio of the first glass microbeads to the second glass microbeads is 6:2-3.

4. The resin-based composite material according to claim 1, characterized in that: The resin matrix includes the following raw materials in parts by weight: 40-50 parts by weight of epoxy resin prepolymer mixture; 15-30 parts by weight of ethylene-octene copolymer; 10-20 parts by weight of nano toughening particles.

5. The resin-based composite material according to claim 4, characterized in that: The epoxy resin prepolymer mixture comprises a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin.

6. The resin-based composite material according to claim 5, characterized in that: When the epoxy resin prepolymer mixture includes bisphenol A epoxy resin, bisphenol F epoxy resin and hydantoin epoxy resin, the weight ratio of the bisphenol A epoxy resin, the bisphenol F epoxy resin and the hydantoin epoxy resin is 2-4:1-3:

1.

7. The resin-based composite material according to claim 4, characterized in that: The weight ratio of the sum of the ethylene-octene copolymer and the nano toughening particles to the epoxy resin prepolymer mixture is 0.65-0.85:

1.

8. A method for preparing a composite material, characterized in that: The method for preparing the composite material is used to prepare the resin-based composite material according to any one of claims 1 to 7, and the method for preparing the composite material comprises: Mixing the resin matrix and the glass microbeads at a first preset temperature to obtain a first mixture; mixing the first mixture with the curing agent at a second preset temperature to obtain a second mixture; impregnating the reinforcing fiber with the second mixture to obtain a prepreg; The prepreg is cured under a preset curing system to obtain the resin-based composite material.

9. The method for preparing a composite material according to claim 8, characterized in that: Before mixing the resin matrix and the glass microspheres at the first preset temperature, the preparation method further comprises: The initial glass microspheres are immersed in an organic solvent and then dried to obtain the glass microspheres.

10. The method for preparing a composite material according to claim 8, characterized in that: The preparation method of the resin matrix comprises: The epoxy resin prepolymer mixture, the ethylene-octene copolymer and the nano toughening particles are mixed at a third preset temperature to obtain the resin matrix.

Citation Information

Cited By

  • Composite material and preparation method thereof

    CN120737548A