Reinforced fiber thermoplastic prepreg, sports equipment blank and forming method of sports equipment blank
By using a composite resin system of bisphenol glycidyl ether type epoxy resin and dihydroxyphenol compound, combined with a catalyst, a moderately viscous reinforcing fiber thermoplastic prepreg is solved, and the molding difficulties and resources of reinforcing fiber prepreg in the prior art are solved. The problem of waste has achieved high mechanical properties and recyclable sports equipment embryo molding.
Patent Information
- Application Number
- CN202410988596.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing reinforced fiber prepregs have poor viscosity and poor molding effect during processing, making it difficult to prepare thermoplastic fiber composite materials of complex shapes, and the thermosetting resin is difficult to recycle and reuse, resulting in waste of resources.
A composite resin system consisting of bisphenol glycidyl ether type epoxy resin and dihydroxyphenol compound is used to combine with a catalyst to form a reinforced fiber thermoplastic prepreg that can maintain moderate viscosity at room temperature, and the in-situ polymerization of sports equipment is formed by high temperature and high pressure The resin polymerization is promoted by catalyst to form a composite interface with high interface strength.
The good viscosity and flexibility of the reinforced fiber thermoplastic prepreg are achieved, which is convenient for manual molding, and the molded sports equipment embryo body has excellent mechanical properties and recyclability, solving the problem of resource waste.
Smart Images

Figure BDA0004958224290000061 
Figure BDA0004958224290000081 
Figure BDA0004958224290000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sports equipment, and in particular, relates to a reinforced fiber thermoplastic prepreg, a sports equipment embryo and a molding method thereof. Background Art
[0002] Reinforced fiber prepreg refers to an intermediate made by impregnating uncured resin in reinforcing fibers. At present, reinforced fiber prepreg has been used in many fields. For example, in the field of automotive products, reinforced fiber prepreg can be used to produce decorative panels and seat support frames in the car. In the field of sporting goods, reinforced fiber prepreg can be used to manufacture high-performance sports equipment such as bicycle frames and racing boats.
[0003] Thermosetting resin is used as the matrix resin for preparing the reinforcing fiber prepreg. The reinforcing fiber prepreg needs to be toughened and modified by the thermosetting resin. In addition, the thermosetting resin also has the disadvantage that it is difficult to recycle the reinforcing fiber compounded with it, resulting in a waste of resources. Compared with thermosetting resin, thermoplastic resin has the advantages of good toughness and easy recycling of the reinforcing fiber compounded with it. At present, the method of using thermoplastic resin as the matrix resin to make reinforcing fiber prepreg is mainly hot melt method or solvent method: the hot melt method is mainly to melt the thermoplastic resin into a viscous liquid by heating and then impregnate the fiber. However, the thermoplastic resin melt has a high melt viscosity, which brings certain difficulties to the impregnation and molding of the reinforcing fiber. In addition, the thermoplastic resin generally has a high melting temperature, so in the process of preparing and processing the reinforcing fiber prepreg, the thermoplastic resin needs to be kept in a melt state and consumes a lot of energy; and the solvent method is to dissolve the thermoplastic resin into a solution by an appropriate solvent, and then use the solution to impregnate the reinforcing fiber, and then remove the solvent in the solution. Since the above methods all directly use thermoplastic resins that already have a high molecular weight to process (melt or dissolve) and impregnate the reinforcing fibers, the reinforcing fiber prepregs obtained thereby are generally non-sticky and hard in texture at room temperature, with poor molding effects, and cannot be manually stacked and bonded to form a blank, making it difficult to produce complex-shaped special-shaped thermoplastic fiber-reinforced composite materials. Summary of the invention
[0004] The object of the present invention is to provide a reinforced fiber thermoplastic prepreg, which has good viscosity (tacky, drop) at room temperature and can be manually stacked and pasted into a sports equipment preform; the sports equipment preform is then in-situ polymerized under high temperature and high pressure to form a sports equipment embryo; thus, the reinforced fiber thermoplastic prepreg can be used to easily and flexibly form sports equipment embryos of various shapes and with good mechanical properties.
[0005] According to a first aspect of the present invention, a reinforced fiber thermoplastic prepreg is provided, which comprises reinforcing fibers and a composite resin system, wherein the composite resin system comprises a bisphenol glycidyl ether type epoxy resin, a dihydric phenol compound, a catalyst and a polar solvent, wherein the weight average molecular weight of the bisphenol glycidyl ether type epoxy resin is 300 to 1000, and the catalyst comprises at least one of a quaternary ammonium catalyst and an organic phosphine catalyst. Based on the component composition of the composite resin system, the composite resin system has low reaction activity at room temperature, will not form polymers with high molecular weight, and can maintain a relatively stable component composition. Based on this, on the one hand, the composite resin system maintains moderate viscosity and can adhere to the surface of the reinforcing fiber, and its viscosity is not too high, which is conducive to the composite resin system to fully spread on the surface of the reinforcing fiber and infiltrate the reinforcing fiber. On the other hand, the reinforced fiber thermoplastic prepreg provided by the present invention will not harden too quickly, and the reinforced fiber thermoplastic prepreg can maintain a wet state and good bendability for a long time. The above two aspects work together to make the reinforced fiber thermoplastic prepreg provided by the present invention easy to transfer and adjust the shape, so that the reinforced fiber thermoplastic prepreg can flexibly adapt to various special-shaped molds and substrates. When the above-mentioned reinforced fiber thermoplastic prepreg is heated, the bisphenol glycidyl ether type epoxy resin component and the dihydric phenol compound component in the composite resin system can undergo a polymerization reaction under the catalytic action of the catalyst component. The mechanism of the polymerization reaction is: under the catalytic action of the catalyst, the epoxy group of the bisphenol glycidyl ether type epoxy resin is ring-opened and undergoes a polymerization reaction with the hydroxyl group of the dihydric phenol compound, thereby obtaining a product including a thermoplastic resin having a chain segment represented by general formula I in its molecular structure, wherein general formula I is The weight average molecular weight of the thermoplastic resin can reach 40,000 to 60,000, and the thermoplastic resin can construct a composite interface with high interface strength together with the reinforcing fiber.
[0006] Preferably, the reinforcing fiber includes at least one of carbon fiber, glass fiber, nylon fiber, Kefka fiber, basalt fiber, and nylon fiber.
[0007] Preferably, in the composite resin system, the molar ratio of epoxy groups contained in the bisphenol glycidyl ether epoxy resin to phenolic hydroxyl groups contained in the hydroxyphenol compound is 0.98 to 1.03:1. When the ratio of the bisphenol glycidyl ether epoxy resin to the dihydric phenol compound in the composite resin system satisfies the above relationship, on the one hand, the wetting effect of the composite resin system on the reinforcing fiber can be improved, and on the other hand, it is beneficial to increase the yield of the advantageous thermoplastic resin, which is reflected in that the sports equipment embryo obtained by molding the reinforcing fiber thermoplastic prepreg has better mechanical properties.
[0008] Preferably, the bisphenol glycidyl ether epoxy resin includes at least one of bisphenol A diglycidyl ether epoxy resin, bisphenol F diglycidyl ether epoxy resin, and bisphenol S diglycidyl ether epoxy resin.
[0009] Preferably, the dihydric phenol compound includes at least one of a bisphenol compound, a condensed polycyclic dihydroxy compound, and a phenol compound having an allyl group.
[0010] Preferably, the dihydric phenol compound includes at least one of bisphenol A, bisphenol F, bisphenol S, dihydroxynaphthalene, diallylresorcinol, diallylbisphenol A, and triallyldihydroxybiphenyl.
[0011] Preferably, the catalyst includes an organic phosphine catalyst and a quaternary ammonium catalyst, the organic phosphine catalyst includes triphenylphosphine, the quaternary ammonium catalyst includes tetrabutylammonium bromide, and the amount of the catalyst is such that the molar ratio of triphenylphosphine to tetrabutylammonium bromide is 1 to 3: 1. Triphenylphosphine and tetrabutylammonium bromide are combined to form a composite catalyst, and under the catalytic action of the composite catalyst, the adhesion of the obtained thermoplastic resin product to the reinforcing fiber material can be maintained at a high level for a long time, which is conducive to the long-term stable compounding of the thermoplastic resin and the reinforcing fiber material.
[0012] According to a second aspect of the present invention, there is provided an application of the above-mentioned reinforced fiber thermoplastic prepreg in manufacturing sports equipment and / or gas cylinders. The sports equipment includes but is not limited to bicycles, electric bicycles, surfboards, rowing oars, water bicycles, etc., and the gas cylinders include but are not limited to industrial gas cylinders, and the industrial gas cylinders include but are not limited to oxygen cylinders and hydrogen cylinders.
[0013] According to a third aspect of the present invention, there is provided a sports equipment embryo, which is composited with reinforcing fibers and a thermoplastic resin; the thermoplastic resin is polymerized from a bisphenol glycidyl ether epoxy resin and a dihydric phenol compound, and the molecular structure of the thermoplastic resin contains a chain segment represented by the following general formula I, wherein the general formula I is In the general formula I, Ar1 and Ar2 are independently selected from aromatic groups containing a benzene ring, n is the degree of polymerization of the chain segment represented by the general formula I, and the weight average molecular weight of the thermoplastic resin is ≥40,000.
[0014] Preferably, the glass transition temperature of the thermoplastic resin is 90 to 130°C.
[0015] Preferably, calculated by mass ratio, the thermoplastic resin: reinforcing fiber = 35-45:55-65.
[0016] According to a fourth aspect of the present invention, a method for molding the above-mentioned sports equipment embryo body is provided, comprising the following operations: step 1, preparing component A and component B respectively, wherein component A is formed by mixing a bisphenol glycidyl ether type epoxy resin and a dihydric phenol compound, and component B includes a catalyst, and the catalyst includes at least one of a quaternary ammonium catalyst and an organic phosphine catalyst; step 2, mixing component A and component B to obtain an impregnation mixture; step 3, impregnating reinforcing fibers into the impregnation mixture to obtain a reinforcing fiber thermoplastic prepreg; step 4, using the reinforcing fiber thermoplastic prepreg to make a preform; step 5, allowing the bisphenol glycidyl ether type epoxy resin and the dihydric phenol compound to undergo a polymerization reaction under the catalytic action of the catalyst, thereby in-situ polymerization on the surface of the reinforcing fibers to generate a thermoplastic resin, so that the preform is converted into a sports equipment embryo body.
[0017] Preferably, component B is a mixed solution obtained by dissolving a catalyst in a polar solution, or component B is a resin mixture obtained by melt-mixing a catalyst and a bisphenol glycidyl ether type epoxy resin.
[0018] Preferably, component B is a resin mixture obtained by melt-mixing a catalyst and a bisphenol glycidyl ether type epoxy resin, and step three is: immersing the reinforcing fiber in the resin mixture to obtain a reinforcing fiber thermoplastic prepreg.
[0019] Preferably, the viscosity of the resin mixture at 40° C. to 100° C. is 30,000 to 100,000 cp.
[0020] Preferably, component B is a mixed solution obtained by dissolving a catalyst in a polar solution, and the mixed solution obtained by mixing component A and component B is the impregnation liquid. Then step three is: immersing the reinforcing fiber in the impregnation liquid to obtain a prepreg semi-finished product, and then volatilizing the polar solvent contained in the prepreg semi-finished product to obtain a reinforcing fiber thermoplastic prepreg.
[0021] The above step three is specifically as follows: the polar solvent contained in the prepreg semi-finished product is volatilized to obtain a reinforced fiber thermoplastic prepreg, and then the reinforced fiber thermoplastic prepreg is cut into required specifications and sizes, and the laminating personnel stack the preforms manually according to the R&D design, and finally the preforms are transferred to the molding mold, the molds are closed after finishing, and then the molding molds are pushed to the molding table.
[0022] Preferably, the viscosity of the impregnation liquid is 80 to 120 cp. Based on the composition of the pre-impregnation liquid, further controlling the viscosity of the pre-impregnation liquid within the above range is beneficial to further improve the wetting effect of the pre-impregnation liquid on the reinforcing fibers.
[0023] Preferably, the polar solvent includes a ketone solvent. Among the available polar solvents, ketone solvents have lower toxicity and are easily volatile. Using ketone solvents as components of the composite resin system is beneficial to the penetration of the composite resin system between the reinforcing fibers and can improve the safety and processing efficiency of the reinforcing fiber thermoplastic prepreg molding.
[0024] Optionally, the polar solvent includes at least one of methyl ethyl ketone, acetone, and butanone.
[0025] Preferably, the polar solvent is methyl ethyl ketone.
[0026] In the above step 5, the polymerization reaction is carried out under high temperature and high pressure.
[0027] Preferably, the process of step 5 comprises: S1. heating the preform to a first temperature at a heating rate of 3-5°C / min, and during the heating process, applying pressure to the preform and increasing the pressure from a first pressure to a second pressure, wherein the first temperature is 100-130°C, the first pressure is 30-60psi, and the second pressure is 120-180psi; S2. when the preform reaches the first temperature, the pressure applied to the preform is suddenly reduced to a third pressure, and the preform is kept at the first temperature and the third pressure for 5-20 minutes, and the third pressure is 30-75psi; S3 .Then the preform is heated from the first temperature to the second temperature at a heating rate of 1 to 4°C / min. During the above heating process, the pressure applied to the preform is increased from the third pressure step to the fourth pressure. The preform is kept warm and pressurized at the second temperature and the fourth pressure for 50 to 120 minutes to obtain a semi-finished product, wherein the second temperature is 140 to 180°C and the fourth pressure is 180 to 240 psi; S4. The semi-finished product is then cooled at a cooling rate of 3 to 5°C / min. During the cooling process, the fourth pressure is kept applied to the semi-finished product. When the temperature drops to 30 to 70°C, the mold is opened to obtain a finished product.
[0028] In the molding process, by adopting specific temperature and pressure control in step five, it is beneficial to further improve the structural stability of the embryo (the reinforcing fibers and the thermoplastic resin are not easy to be separated) and the mechanical properties of the embryo. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. In the following embodiments, the molding equipment used to mold the sports equipment special-shaped embryo body involved is the composite material workpiece molding equipment described in the prior invention patent application text of Dongguan Taihe Composite Materials Co., Ltd. with publication number CN112721078A.
[0030] Example 1
[0031] 1. Preparation of reinforced fiber thermoplastic prepreg
[0032] In this embodiment, a composite resin system and reinforcing fibers are used to prepare a reinforced fiber thermoplastic prepreg. The composite resin system is composed of a reactive monomer and a catalyst. Specifically, the reactive monomer includes a bisphenol glycidyl ether type epoxy resin and a dihydric phenol compound. In this embodiment, different treatment groups and control groups are set up with the types of reactive monomers and catalysts included in the composite resin system as variables. The composition of the composite resin system corresponding to each group is shown in Table 1. "Mw" in Table 1 represents the weight average molecular weight of the corresponding material.
[0033] Table 1. Types and ratios of reactive monomers used in the preparation of thermoplastic resins in each treatment group of this embodiment
[0034]
[0035] The treatment group and the control group shown in Table 1 were prepared in the following manner:
[0036] S1. Preparation of composite resin system
[0037] S1.1 Preparation of Component A
[0038] Each treatment group corresponds to Table 1. The bisphenol glycidyl ether type epoxy resin and dihydric phenol compound used in each treatment group are weighed according to the amount. The amount of bisphenol glycidyl ether type epoxy resin used is 100g, and the amount of dihydric phenol compound used is determined according to the ratio of epoxy group contained in bisphenol glycidyl ether type epoxy resin to phenolic hydroxyl group contained in hydroxyphenol compound = 1:1. Then, the bisphenol glycidyl ether type epoxy resin used is heated to about 120°C, and then the dihydric phenol compound is added thereto, and the two are fully stirred until they are uniformly miscible, thereby obtaining component A, and the temperature of component A is reduced to room temperature for standby use.
[0039] S1.2 Preparation of component B:
[0040] Triphenylphosphine and tetrabutylammonium bromide are used as catalysts, the mass of triphenylphosphine is 1% of the total mass of component A, tetrabutylammonium bromide is taken according to the mass ratio of triphenylphosphine to tetrabutylammonium bromide of 2:1, methyl ethyl ketone (MEK) is used as a polar solvent, 40g of MEK is weighed, and then triphenylphosphine and tetrabutylammonium bromide are added thereto, so that the above two catalysts are dissolved and fully dispersed in MEK to form a uniform solution, and component B is prepared for standby use. All treatment groups set in this embodiment prepare component B in the above manner.
[0041] S1.3 Mixing
[0042] Component A and component B are mixed, and the mixed slurry is stirred at a low speed first and then at a high speed until the mixture is uniformly mixed to obtain a prepreg containing a composite resin system, wherein the viscosity of the prepreg is 80-120 cp.
[0043] S2. Preparation of reinforced fiber thermoplastic prepreg
[0044] The prepreg solution is passed into an impregnation tank, and a traction device is used to pull the reinforcing fibers (the reinforcing fibers used in each treatment group of this embodiment are carbon fibers, and the manufacturer and product brand are Toray-T700) into the impregnation tank to be impregnated with the prepreg solution to obtain a prepreg semi-finished product, and then the prepreg semi-finished product is placed in an internal and external circulation drying room to naturally dry the prepreg semi-finished product so that the MEK therein can be fully volatilized, thereby obtaining a reinforced fiber thermoplastic prepreg. During the above impregnation process, the tension of the traction device and the roller position are adjusted to control the impregnation amount of the composite resin system to reach 40wt% of the reinforced fiber thermoplastic prepreg, and the drum speed of the traction device is adjusted to control the unit area weight of the reinforcing fibers in the reinforced fiber thermoplastic prepreg to reach 170g / m 2 .
[0045] 2. Performance test of reinforced fiber thermoplastic prepreg
[0046] (1) Test object:
[0047] The reinforced fiber thermoplastic prepreg samples prepared in each treatment group and control group of this embodiment were sampled and tested for viscosity and bendability.
[0048] (2) Test items and test methods
[0049] Adhesiveness (tacky, drop) test of reinforced fiber thermoplastic prepreg: At 25℃±2℃, 50%±2%RH, two sheets of prepreg provided by the same treatment group or control group are laminated face to face, and then lightly pressed with a roller to make the two laminated. The bonding state of the obtained laminate is used to judge. The specific rating indicators and representative symbols are as follows:
[0050] ○: Not easy to peel off
[0051] ×: Easy to peel off
[0052] ▲: Between the two, can be peeled off.
[0053] Bendability test of reinforced fiber thermoplastic prepreg: At 25℃±2℃, 50%±2%RH, laminate the reinforced fiber thermoplastic prepreg on the surface of the same shaped special-shaped substrate, and judge by observing the bending and fracture of the reinforced fiber thermoplastic prepreg. The specific rating indicators and representative symbols are as follows:
[0054] ○: Easy to bend, and the fibers will not break when laminated on the surface of a special-shaped substrate.
[0055] ×: Difficult to bend. The prepreg is relatively hard. When laminated on the surface of a special-shaped substrate, the fibers break.
[0056] ▲: Although it is a little harder to bend than "○", the fibers will not break when laminated on the surface of a special-shaped base material.
[0057] (3) Test results
[0058] The test results are shown in Table 2. In the test groups, the resin component used to prepare the pre-dip solution is composed of bisphenol glycidyl ether type epoxy resin and dihydric phenol compound, and the above resin component has low reaction activity under room temperature conditions, so that the pre-dip solution prepared by using the above resin component can maintain a stable component composition under room temperature operating conditions. Among them, the weight average molecular weight of the bisphenol glycidyl ether type epoxy resin used in the treatment group 1A, the treatment group 2A, and the treatment group 3A of Example 1 is within the range of 300 to 1000, so that in the process of using the above-mentioned treatment group to prepare the prepreg to impregnate the reinforcing fiber, the viscosity of the prepreg can be maintained within a moderate range, which can not only fully wet the reinforcing fiber, but also spread evenly on the surface of the reinforcing fiber. After the solvent in the prepreg evaporates, the composite resin system remaining in the prepreg can maintain appropriate viscosity, so that it can not only firmly adhere to the surface of the reinforcing fiber, so that the prepreg has excellent viscosity, but also can make the reinforcing fiber thermoplastic prepreg maintain good bendability, thereby making the test objects provided by the treatment group 1A, the treatment group 2A, and the treatment group 3A of Example 1 respectively convenient to transfer and adjust the shape, and have excellent molding operability. However, the weight-average molecular weight of the bisphenol glycidyl ether type epoxy resin used in the composite resin system prepared in Control Group 1 and Control Group 2 of Example 1 is relatively high, resulting in a significantly worse impregnation effect of the prepreg on the reinforcing fiber compared to the prepreg of other treatment groups, and the viscosity of the composite resin system and its uniform distribution on the surface of the reinforcing fiber are also significantly deteriorated, thereby reducing the viscosity of the corresponding reinforcing fiber thermoplastic prepreg.
[0059] Table 2. Performance test results of the reinforced fiber thermoplastic prepreg of Example 1
[0060]
[0061] 3. Preparation of Exosome-specific Embryoid Bodies
[0062] The reinforced fiber thermoplastic prepregs prepared in each treatment group and the control group of this embodiment were respectively transferred to molding molds of the same shape as preforms, and the preforms were subjected to the following operations to form them into sports equipment special-shaped embryos:
[0063] S1. The preform is heated to a first temperature at a heating rate of 5°C / min. During the heating process, pressure is applied to the preform and the pressure is increased from a first pressure to a second pressure, wherein the first temperature is 120°C, the first pressure is 45 psi, and the second pressure is 150 psi;
[0064] S2. When the preform reaches the first temperature, the pressure applied to the preform is suddenly reduced to a third pressure, and the first temperature and the third pressure are maintained at the temperature and the third pressure for 10 minutes, and the third pressure is 45 psi;
[0065] S3. Then, the preform is heated from the first temperature to the second temperature at a heating rate of 3°C / min. During the heating process, the pressure applied to the preform is increased from the third pressure to the fourth pressure, and the preform is kept at the second temperature and the fourth pressure for 90 minutes to obtain a semi-finished product, wherein the second temperature is 150°C and the fourth pressure is 225psi;
[0066] S4. Then the semi-finished product is cooled at a cooling rate of 5°C / min. During the cooling process, the fourth pressure is applied to the semi-finished product. When the temperature drops to 40°C, the mold is opened to obtain a finished product.
[0067] The finished product of the sports equipment special-shaped embryo obtained by the above operation is composited with reinforcing fiber and thermoplastic resin, wherein the weight average molecular weight of the thermoplastic resin is 40000-60000, and the mass percentage of the thermoplastic resin in the sports equipment special-shaped embryo is about 40%.
[0068] 4. Performance test of sports equipment heteromorphic embryos
[0069] (1) Test object
[0070] The sports equipment heteromorphic embryos prepared from the treatment groups and the control group of this example were used as test objects.
[0071] (2) Test items and test methods
[0072] Flexural strength: ASTM D7264-15 (composite material three-point bending test).
[0073] Interlaminar shear strength: ASTM D2344-16 (interlaminar shear test for composite materials).
[0074] Impact properties: ISO 179-1.
[0075] (3) Test results
[0076] The test results of this test example are shown in Table 3. In the process of forming the sports equipment special-shaped body involved in Example 1, by heating the reinforced fiber thermoplastic prepreg, the bisphenol glycidyl ether type epoxy resin and dihydric phenol compound components included therein can undergo polymerization reaction under the catalytic action of the catalyst to generate the chain segments shown in the general formula I in the molecular structure. After the thermoplastic resin is cured, the sports equipment special-shaped body is formed. The above general formula I is Wherein, Ar1 and Ar2 represent aromatic groups containing benzene rings, and n is the degree of polymerization of the chain segment shown in general formula I. From the test results shown in Table 3, it can be seen that among the test objects, the mechanical properties of the sports equipment heteromorphic embryos provided by treatment group 1A, treatment group 2A, and treatment group 3A in Example 1 are significantly better, and the weight average molecular weight of the thermoplastic resins prepared by these treatment groups is within the range of 40,000 to 60,000. Such thermoplastic resins can construct a composite interface with high interface strength together with the reinforcing fibers, while the sports equipment heteromorphic embryos prepared by control group 1 and control group 2 in Example 1 are poor in bending strength, interlaminar shear strength, and impact performance.
[0077] Table 3. Performance test results of the sports equipment heteromorphic embryos of Example 1
[0078] Sports equipment heteromorphic embryo group Bending strength / MPa Interlaminar shear strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 1400 80 240 Example 1 Treatment Group 2A 1300 75 220 Example 1 Treatment Group 3A 1240 76 232 Example 1 Control group 1 1130 68 183 Example 1 Control group 2 1140 65 180
[0079] Example 2
[0080] 1. Preparation of reinforced fiber thermoplastic prepreg
[0081] This embodiment uses the treatment group 1A of Example 1 as a reference, and adopts the composite resin system and the reinforcing fiber to prepare the reinforcing fiber thermoplastic prepreg. Referring to the treatment group 1A of Example 1, this embodiment uses the ratio of bisphenol glycidyl ether type epoxy resin and dihydric phenol compound used in each treatment group as a variable, and sets different treatment groups, which are numbered as treatment group 1B and treatment group 2B, respectively. The specific variable settings are shown in Table 4. In addition to the variables shown in Table 4, the other materials and operations used to prepare the reinforcing fiber thermoplastic prepreg in the treatment groups 1B and 2B set in this embodiment are strictly consistent with those in the treatment group 1A of Example 1.
[0082] Table 4. The usage of monomers for preparing thermoplastic resin reaction in each treatment group of this embodiment
[0083]
[0084]
[0085] 2. Performance test of reinforced fiber thermoplastic prepreg
[0086] (1) Test object:
[0087] The reinforced fiber thermoplastic prepreg samples prepared in treatment group 1A of Example 1 and each treatment group of this example were sampled for viscosity test and bendability test.
[0088] (2) Test items and test methods
[0089] Viscosity test of reinforced fiber thermoplastic prepreg: The viscosity test method and rating index of the reinforced fiber thermoplastic prepreg involved in Example 1 are the same.
[0090] Bendability test of reinforced fiber thermoplastic prepreg: The bendability test method and rating index of the reinforced fiber thermoplastic prepreg involved in Example 1 are the same.
[0091] (3) Test results
[0092] The test results are shown in Table 5. The resin component compositions used in the treatment group 1A of Example 1, the treatment group 1B of Example 2, and the treatment group 2B of Example 2 are different, so that the impregnation effect of the prepreg on the reinforcing fiber is also different. In the treatment group 1A of Example 1, the amount of the bisphenol glycidyl ether type epoxy resin and the hydroxyphenol compound satisfies the epoxy group contained in the bisphenol glycidyl ether type epoxy resin: the phenolic hydroxyl group contained in the hydroxyphenol compound = 1:1, and the prepreg obtained thereby has the best impregnation effect on the reinforcing fiber. The reinforcing fiber thermoplastic prepreg prepared using the prepreg has excellent viscosity and bendability.
[0093] Table 5. Performance test results of the reinforced fiber thermoplastic prepreg of Example 2
[0094]
[0095]
[0096] 3. Preparation of Exosome-specific Embryoid Bodies
[0097] The reinforced fiber thermoplastic prepregs prepared in the treatment groups and the control group of this embodiment were respectively used to prepare special-shaped embryos for sports equipment according to the method for preparing special-shaped embryos for sports equipment in Example 1. Except for the different reinforced fiber thermoplastic prepregs used, all operations in the process of preparing the special-shaped embryos for sports equipment in this embodiment were strictly consistent with those in Example 1.
[0098] 4. Performance test of sports equipment heteromorphic embryos
[0099] (1) Test object
[0100] The sports equipment heteromorphic embryos prepared by the treatment group 1A of Example 1 and the treatment groups of this example were used as test objects.
[0101] (2) Test items and test methods
[0102] Flexural strength: ASTM D7264-15 (composite material three-point bending test).
[0103] Interlaminar shear strength: ASTM D2344-16 (interlaminar shear test for composite materials).
[0104] Impact properties: ISO 179-1.
[0105] (3) Test results
[0106] The test results of this test example are shown in Table 6. It can be seen that among the test objects, the sports equipment special-shaped embryo body prepared by treatment group 1A of Example 1 has the best mechanical properties. On the one hand, the prepreg prepared by treatment group 1A of Example 1 has the best impregnation effect on the reinforced substrate, and the thermoplastic resin can be evenly and firmly attached to the surface of the reinforcing fiber. On the other hand, the resin components contained in the reinforcing fiber thermoplastic prepreg meet a specific ratio, which is beneficial to improve the yield of the resin with mechanical performance advantages, so that the mechanical properties of the sports equipment special-shaped embryo body show advantages in bending strength, interlaminar shear strength, impact performance and other aspects.
[0107] Table 6. Performance test results of the sports equipment heteromorphic embryos of Example 2
[0108] Sports equipment heteromorphic embryo group Bending strength / MPa Interlaminar shear strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 1400 80 240 Example 2 Treatment Group 1B 1370 76 230 Example 2 Treatment Group 2B 1350 72 210
[0109] Example 3
[0110] 1. Preparation of reinforced fiber thermoplastic prepreg
[0111] This embodiment uses the treatment group 1A of Example 1 as a reference, and uses a composite resin system and reinforcing fibers to prepare a reinforced fiber thermoplastic prepreg. Referring to the treatment group 1A of Example 1, this embodiment uses the catalyst composition used to prepare the thermoplastic resin as a variable to set different treatment groups. According to the different catalysts used, treatment group 1C, treatment group 2C, treatment group 3C, and treatment group 4C are set. The specific composition of the catalyst used in each treatment group is shown in Table 7, and the total mass of the catalyst used between each treatment group is controlled to be equal. In the process of preparing the thermoplastic resin in each treatment group of this embodiment, except for the variables shown in Table 7, the other materials and operations used to prepare the reinforced fiber thermoplastic prepreg are strictly consistent with the treatment group 1A of Example 1.
[0112] Table 7. Catalyst compositions used in the preparation of thermoplastic resins in each treatment group of this example
[0113] Group Catalyst composition Example 1 Treatment Group 1A Triphenylphosphine:tetrabutylammonium bromide = 2:1 (mass ratio) Example 3 Treatment Group 1C Triphenylphosphine:tetrabutylammonium bromide = 4:1 (mass ratio) Example 3 Treatment Group 2C Triphenylphosphine:tetrabutylammonium bromide = 0.5:1 (mass ratio) Example 3 Treatment Group 3C Single component: triphenylphosphine Example 3 Treatment Group 4C Single component: Tetrabutylammonium bromide
[0114] 2. Performance test of reinforced fiber thermoplastic prepreg
[0115] (1) Test object:
[0116] The reinforced fiber thermoplastic prepreg samples prepared in treatment group 1A of Example 1 and each treatment group of this example were sampled for viscosity test and bendability test.
[0117] (2) Test items and test methods
[0118] Viscosity test of reinforced fiber thermoplastic prepreg: The viscosity test method and rating index of the reinforced fiber thermoplastic prepreg involved in Example 1 are the same.
[0119] Bendability test of reinforced fiber thermoplastic prepreg: The bendability test method and rating index of the reinforced fiber thermoplastic prepreg involved in Example 1 are the same.
[0120] (3) Test results
[0121] The test results are shown in Table 8. The difference in material composition between the reinforced fiber thermoplastic prepregs tested in this test example lies in the different catalyst compositions contained in the composite resin system. From the test results shown in Table 8, it can be seen that the reinforced fiber thermoplastic prepregs prepared using catalysts with different components also have certain differences in viscosity and flexibility.
[0122] Table 8. Performance test results of the reinforced fiber thermoplastic prepreg of Example 3
[0123]
[0124] 3. Preparation of Exosome-specific Embryoid Bodies
[0125] The reinforced fiber thermoplastic prepregs prepared in the treatment groups and the control group of this embodiment were respectively used to prepare special-shaped embryos for sports equipment according to the method for preparing special-shaped embryos for sports equipment in Example 1. Except for the different reinforced fiber thermoplastic prepregs used, all operations in the process of preparing the special-shaped embryos for sports equipment in this embodiment were strictly consistent with those in Example 1.
[0126] 4. Performance test of sports equipment heteromorphic embryos
[0127] (1) Test object
[0128] The sports equipment heteromorphic embryos prepared by the treatment group 1A of Example 1 and the treatment groups of this example were used as test objects.
[0129] (2) Test items and test methods
[0130] Flexural strength: ASTM D7264-15 (composite material three-point bending test).
[0131] Interlaminar shear strength: ASTM D2344-16 (interlaminar shear test for composite materials).
[0132] Impact properties: ISO 179-1.
[0133] (3) Test results
[0134] The test results of this test example are shown in Table 9. The experimental results show that the composite fiber thermoplastic prepregs tested can all be used to produce molded sports equipment heterogeneous embryos, which shows that triphenylphosphine and tetrabutylammonium bromide can be used as single-component catalysts or as a combined catalyst to effectively catalyze the polymerization reaction of the resin components in the composite fiber thermoplastic prepreg and convert them into thermoplastic resins. However, compared with Example 3 Treatment Group 3C using triphenylphosphine as a single-component catalyst and Example 3 Treatment Group 4C using tetrabutylammonium bromide as a single-component catalyst, the bending strength, interlaminar shear strength, and impact performance of the sports equipment heterogeneous embryos produced by Example 1 Treatment Group 1A, Example 3 Treatment Group 1C, and Example 3 Treatment Group 2C using triphenylphosphine and tetrabutylammonium bromide as a combined catalyst are all improved. This shows that in the molding process of the heterogeneous embryo body of sports equipment, the combined catalytic effect of triphenylphosphine and tetrabutylammonium bromide on the resin system is beneficial to further improve the comprehensive mechanical properties of the heterogeneous embryo body of the sports equipment. From the test results shown in Table 9, it can be seen that when the dosage ratio of triphenylphosphine and tetrabutylammonium bromide reaches triphenylphosphine:tetrabutylammonium bromide = 2:1, the comprehensive mechanical properties of the heterogeneous embryo body of the sports equipment obtained in this way are optimal.
[0135] Table 9. Performance test results of the sports equipment heteromorphic embryos of Example 3
[0136] Sports equipment heteromorphic embryo group Bending strength / MPa Interlaminar shear strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 1400 80 240 Example 3 Treatment Group 1C 1380 76 230 Example 3 Treatment Group 2C 1360 72 210 Example 3 Treatment Group 3C 1250 80 260 Example 3 Treatment Group 4C 1320 70 210
[0137] Example 4
[0138] 1. Preparation of reinforced fiber thermoplastic prepreg
[0139] The materials and specific methods for preparing the reinforced fiber thermoplastic prepreg in this embodiment are completely consistent with those of treatment group 1A in Example 1.
[0140] 2. Preparation of reinforced fiber thermoplastic prepreg shaped blank
[0141] The reinforced fiber thermoplastic prepreg prepared in this embodiment is used to prepare reinforced fiber thermoplastic prepreg shaped blanks in different molding methods. Different processing groups are set according to different molding methods, and are numbered as processing group 1D, processing group 2D, processing group 3D, and processing group 4D.
[0142] (1) Treatment group 1D was prepared by the following method:
[0143] S1. The preform is heated to 150°C at a heating rate of 5°C / min, and during the heating process, pressure is applied to the preform and the pressure is increased from a first pressure step to a second pressure, the first pressure is 45 psi, and the second pressure is 150 psi;
[0144] S2. When the preform reaches 150°C, the pressure applied to the preform is suddenly reduced to the third pressure, and the preform is kept at 150°C and the third pressure for 10 minutes, and the third pressure is 45 psi;
[0145] S3. Then, the pressure applied to the preform is increased from the third pressure step to the fourth pressure step, and the preform is kept at 150°C and the fourth pressure for 90 minutes to obtain a semi-finished product, wherein the fourth pressure is 225 psi;
[0146] S4. Then the semi-finished product is cooled at a cooling rate of 5°C / min. During the cooling process, the fourth pressure is applied to the semi-finished product. When the temperature drops to 40°C, the mold is opened to obtain a finished product.
[0147] (2) Treatment group 2D completed the preparation of sports equipment heteromorphic embryos in the following manner:
[0148] S1. The preform is heated to a first temperature at a heating rate of 5°C / min, and during the heating process, pressure is applied to the preform and the pressure is increased from 45 psi to 225 psi in steps, wherein the first temperature is 120°C;
[0149] S2. When the preform reaches the first temperature, the preform is kept at the first temperature and pressure of 225 psi for 10 minutes;
[0150] S3. Continue to apply 225 psi pressure to the preform, then heat the preform from the first temperature to the second temperature at a heating rate of 3 ° C / min, and keep the temperature and pressure at the second temperature and 225 psi pressure for 90 minutes to obtain a semi-finished product, wherein the second temperature is 150 ° C;
[0151] S4. Then the semi-finished product is cooled at a cooling rate of 5°C / min. During the cooling process, the fourth pressure is applied to the semi-finished product. When the temperature drops to 40°C, the mold is opened to obtain a finished product.
[0152] (3) Treatment group 3D completed the preparation of sports equipment heteromorphic embryos in the following manner:
[0153] S1. The preform is heated to a first temperature at a heating rate of 5°C / min, and during the heating process, pressure is applied to the preform and the pressure is increased from 45 psi to 150 psi in steps, wherein the first temperature is 120°C;
[0154] S2. When the preform reaches the first temperature, the preform is kept at the first temperature and pressure of 150 psi for 10 minutes;
[0155] S3. Then, the preform is heated from the first temperature to the second temperature at a heating rate of 3°C / min. During the heating process, the pressure applied to the preform is increased from 150 psi to 225 psi in a stepwise manner. The preform is kept at the second temperature and the pressure of 225 psi for 90 minutes to obtain a semi-finished product, wherein the second temperature is 150°C;
[0156] S4. Then the semi-finished product is cooled at a cooling rate of 5°C / min. During the cooling process, a pressure of 225 psi is applied to the semi-finished product. When the temperature drops to 40°C, the mold is opened to obtain a finished product.
[0157] (4) Treatment group 4D completed the preparation of sports equipment heteromorphic embryos in the following manner:
[0158] S1. The preform is heated to a first temperature at a heating rate of 5°C / min. During the heating process, pressure is applied to the preform and the pressure is increased from a first pressure to a second pressure, wherein the first temperature is 120°C, the first pressure is 45 psi, and the second pressure is 150 psi;
[0159] S2. When the preform reaches the first temperature, the pressure applied to the preform is suddenly reduced to a third pressure, and the first temperature and the third pressure are maintained at the temperature and the third pressure for 10 minutes, and the third pressure is 45 psi;
[0160] S3. Then, the preform is heated from the first temperature to the second temperature at a heating rate of 3°C / min. During the heating process, the pressure applied to the preform is increased from the third pressure to the fourth pressure, and the preform is kept at the second temperature and the fourth pressure for 90 minutes to obtain a semi-finished product, wherein the second temperature is 150°C and the fourth pressure is 225psi;
[0161] S4. Then, the semi-finished product is cooled naturally, and the pressure applied to the semi-finished product is stopped during the cooling process. When the temperature drops to 40°C, the mold is opened to obtain the finished product.
[0162] 3. Performance test of sports equipment heteromorphic embryos
[0163] (1) Test object
[0164] The sports equipment heteromorphic embryos prepared by the treatment group 1A of Example 1 and the treatment groups of this example were used as test objects.
[0165] (2) Test items and test methods
[0166] Flexural strength: ASTM D7264-15 (composite material three-point bending test).
[0167] Interlaminar shear strength: ASTM D2344-16 (interlaminar shear test for composite materials).
[0168] Impact properties: ISO 179-1.
[0169] (3) Test results
[0170] The test results of this test example are shown in Table 10. As described above, the prepreg components used in the treatment group 1A of implementation 1 and the treatment groups 1D, 2D, 3D, and 4D of embodiment 4 are the same, the types of reinforcing fibers are the same, and the material compositions of the reinforcing fiber thermoplastic prepregs prepared by the above treatment groups are also exactly the same, however, the specific processes of the above treatment groups using the reinforcing fiber thermoplastic prepregs to form the special-shaped embryos of sports equipment constitute differences. The process of molding the sports equipment special-shaped embryos of treatment group 1A in Example 1 is used as a reference for comparison: the process of molding the sports equipment special-shaped embryos of treatment group 1D in Example 4 does not use a complete gradient temperature control process, and the molding temperature is controlled at 150°C for a long time during the molding process (equivalent to the "second temperature" of treatment group 1A in Example 1 in the process of preparing the sports equipment special-shaped embryos); the process of molding the sports equipment special-shaped embryos of treatment group 2D in Example 4 does not use a complete gradient pressure control process, and the pressure is controlled at 225psi for a long time during the molding process (equivalent to the "fourth pressure" of treatment group 1A in Example 1 in the process of preparing the sports equipment special-shaped embryos); treatment group 3D in Example 4 omits the operation of causing a sudden change in pressure in S2; treatment group 4D in Example 4 omits the operation of temperature control and pressure holding treatment in the cooling process of S4. It can be seen from the test results shown in Table 10 that the mechanical properties of sports equipment special-shaped embryos prepared by different molding methods are different. Among the tested special-shaped embryos of sports equipment, the special-shaped embryos of sports equipment prepared by treatment group 1A of Example 1 showed advantages in bending strength, interlaminar shear strength and impact performance.
[0171] Table 10. Performance test results of the sports equipment heteromorphic embryos of Example 4
[0172] Sports equipment heteromorphic embryo group Bending strength / MPa Interlaminar shear strength / MPa <![CDATA[Impact performance / (KJ / m 2 )]]> Example 1 Treatment Group 1A 1400 80 240 Example 4 Treatment Group 1D 1250 75 190 Example 4 Treatment Group 2D 1350 78 220 Example 4 Treatment Group 3D 1180 70 210 Example 4 Treatment Group 4D 1230 72 205
[0173] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A reinforced fiber thermoplastic prepreg, characterized in that: The reinforced fiber thermoplastic prepreg comprises reinforcing fibers and a composite resin system, wherein the composite resin system comprises a bisphenol glycidyl ether type epoxy resin, a dihydric phenol compound and a catalyst, wherein the weight average molecular weight of the bisphenol glycidyl ether type epoxy resin is 300 to 1000, and the catalyst comprises at least one of a quaternary ammonium catalyst and an organic phosphine catalyst.
2. The reinforced fiber thermoplastic prepreg according to claim 1, characterized in that: In the composite resin system, calculated by molar ratio, the epoxy groups contained in the bisphenol glycidyl ether epoxy resin: the phenolic hydroxyl groups contained in the dihydric phenol compound = 0.98 to 1.03:
1.
3. The reinforced fiber thermoplastic prepreg according to claim 1, characterized in that: The catalyst includes the organic phosphine catalyst and the quaternary ammonium catalyst, the organic phosphine catalyst includes triphenylphosphine, the quaternary ammonium catalyst includes tetrabutylammonium bromide, and the amount of the catalyst is such that the molar ratio of the triphenylphosphine to the tetrabutylammonium bromide is 1 to 3:
1.
4. Use of the reinforced fiber thermoplastic prepreg according to any one of claims 1 to 3 in the production of sports equipment and / or gas cylinders.
5. A sports equipment embryo, characterized in that: The embryo is composited with reinforcing fibers and thermoplastic resin; the thermoplastic resin is polymerized from bisphenol glycidyl ether epoxy resin and dihydric phenol compound, and the molecular structure of the thermoplastic resin contains the chain segment shown in the following general formula I, wherein the general formula I is In the general formula I, Ar1 and Ar2 are independently selected from aromatic groups containing a benzene ring, n is the degree of polymerization of the chain segment represented by the general formula I, and the weight average molecular weight of the thermoplastic resin is ≥40,000.
6. The sports equipment embryo as claimed in claim 5, characterized in that: The glass transition temperature of the thermoplastic resin is 90 to 130°C.
7. The sports equipment embryo as claimed in claim 5, characterized in that: Calculated by mass ratio, the thermoplastic resin: the reinforcing fiber = 35-45:55-65.
8. The method for forming a sports equipment embryo as claimed in any one of claims 5 to 7, characterized in that: The following operations are included: Then, a preform is prepared by using the reinforced fiber thermoplastic prepreg; Step 1, preparing component A and component B respectively, wherein the component A is formed by mixing the bisphenol glycidyl ether epoxy resin and the dihydric phenol compound, and the component B includes a catalyst, and the catalyst includes at least one of a quaternary ammonium catalyst and an organic phosphine catalyst; Step 2, mixing the component A and the component B to obtain an impregnated mixture; Step three, immersing the reinforcing fiber into the impregnation mixture to obtain a reinforcing fiber thermoplastic prepreg; Step 4, using the reinforced fiber thermoplastic prepreg to make a preform; Step 5: Allow the bisphenol glycidyl ether epoxy resin and the dihydric phenol compound to undergo a polymerization reaction under high temperature and high pressure conditions under the catalytic action of the catalyst, thereby in situ polymerizing the thermoplastic resin on the surface of the reinforcing fiber, so that the preform is converted into the sports equipment embryo.
9. The method for forming a sports equipment embryo as claimed in claim 8, characterized in that: The B component is a mixed solution obtained by dissolving the catalyst in a polar solution, or the B component is a resin mixture obtained by melt-mixing the catalyst and a bisphenol glycidyl ether type epoxy resin.
10. The method for forming a sports equipment embryo as claimed in claim 9, characterized in that: The polar solvent includes a ketone solvent.
11. The method for forming a sports equipment embryo as claimed in any one of claims 8 to 10, characterized in that: The process of step five includes: S1. The preform is heated to a first temperature at a heating rate of 3 to 5°C / min. During the heating process, pressure is applied to the preform and the pressure is increased from a first pressure to a second pressure, wherein the first temperature is 100 to 130°C, the first pressure is 30 to 60 psi, and the second pressure is 120 to 180 psi; S2. When the preform reaches the first temperature, the pressure applied to the preform is suddenly reduced to a third pressure, and the first temperature and the third pressure are maintained for 5 to 20 minutes, and the third pressure is 30 to 75 psi; S3. Then, the preform is heated from the first temperature to the second temperature at a heating rate of 1 to 4°C / min. During the heating process, the pressure applied to the preform is increased from the third pressure to the fourth pressure. The preform is kept at the second temperature and the fourth pressure for 50 to 120 minutes to obtain a semi-finished product, wherein the second temperature is 140 to 180°C and the fourth pressure is 180 to 240 psi. S4. Then, the semi-finished product is cooled at a cooling rate of 3 to 5°C / min, and the fourth pressure is applied to the semi-finished product during the cooling process. When the temperature drops to 30 to 70°C, the mold is opened to obtain a finished product.