High-extension and high-resilience TPU color-changing film and preparation method thereof

By using a combination of aliphatic polyurethane and thermoplastic polyester elastomers with hardness of 45A-60A in the TPU color change film, the problem of insufficient ductility and resilience of the existing TPU color change film was solved, and high ductility and The high-resilience color-changing film improves its application performance.

CN118909427AInactive Publication Date: 2024-11-08JIANGSU YAOSHENG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411003719.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing TPU color-changing film has poor ductility and resilience, which limits its application performance in actual use.

Method used

Using a combination of aliphatic polyurethane, thermoplastic polyester elastomer with a hardness of 45A-60A, polyethylene terephthalate fiber and other materials, a high-release and high-resilience TPU color modification is prepared through specific ratios and preparation processes. membrane.

Benefits of technology

It achieves high ductility and high rebound in continuous cracking under the action of large external forces, and improves the service life and application performance of the TPU color-changing film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909427A_ABST
    Figure CN118909427A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of color alteration films, and provides a high-extension and high-resilience TPU color alteration film and a preparation method thereof. The TPU color-changing film is prepared from the following raw materials in parts by weight: 30-45 parts of aliphatic polyurethane, 20-40 parts of thermoplastic polyester elastomer with the hardness of 45A-60A, 10-40 parts of polyethylene terephthalate fiber, 4-12 parts of pigment, 2-5 parts of ultraviolet light absorber, 1-5 parts of antioxidant stabilizer, 1-5 parts of dispersing agent, 5-8 parts of filler and 10-15 parts of solvent. Compared with the prior art, the TPU color-changing film disclosed by the invention contains the thermoplastic polyester elastomer with the hardness of 45A-60A on the basis of containing aliphatic polyurethane, has the combination of various high-molecular polymers, changes the chemical formula of substances, can extend and does not break under the action of a relatively large external force, and can be used for preparing the color-changing film. The prepared TPU color changing film can have high ductility; and the polyethylene terephthalate fibers are added into the prepared components, so that the TPU color-changing film also has high rebound resilience by utilizing the high strength and the elastic recovery capability of the polyethylene terephthalate fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of color-changing films, and in particular relates to a high-extensibility and high-rebound TPU color-changing film and a preparation method thereof. Background Art

[0002] With the continuous development of my country's economy and the continuous improvement of people's living standards. Invisible car cover, as the new favorite in the car beauty industry, has been recognized by many domestic consumers. The number of cars in use and the number of new cars have brought huge potential market space for invisible car cover. Car body color-changing film (invisible car cover) is a service that uses a film with rich and diverse colors to change the appearance of the entire car or part of the car by covering and pasting it as a whole; the car body color-changing film is mainly attached to the surface of the car body through polymer materials and is easy to remove; the mainstream car body color-changing film products include: transparent film, car electroplating film, pearlescent film, glossy film, matte film, painted film, leather grain film, brushed film, electroplating film, electro-optical metal film, matte metal film (referred to as matte ice film).

[0003] In the relevant prior art, for example, the Chinese invention patent application is titled "A TPU color-changing film and its preparation method", with publication number CN115895490A, and the specific disclosed scheme is "The TPU color-changing film is a multi-layer film composite layered structure, which includes a protective film, a repair coating, a dispersed surface color layer, a base color layer, an installation adhesive layer and a release film arranged in sequence from top to bottom."; Although this color-changing film has a long service life, strong anti-scratch and anti-collision capabilities, high brightness, strong stain resistance, impact resistance, and good weather resistance; but in actual use, it was found that due to the limitations of the internal structure, the ductility and resilience of this color-changing film are poor. Summary of the Invention

[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a high-extensibility and high-resilience TPU color-changing film and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-extensibility and high-rebound TPU color-changing film, which is made according to the weight parts of the following raw materials:

[0007] 30-45 parts of aliphatic polyurethane, 20-40 parts of thermoplastic polyester elastomer with a hardness of 45A-60A, 10-40 parts of polyethylene terephthalate fiber, 4-12 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, 1-5 parts of dispersant, 5-8 parts of filler, and 10-15 parts of solvent.

[0008] As a preferred technical solution of the present invention, the TPU color-changing layer is calculated based on the weight parts of the following raw materials:

[0009] 32 parts of aliphatic polyurethane, 22 parts of thermoplastic polyester elastomer with a hardness of 55A, 15 parts of polyethylene terephthalate fiber, 6 parts of pigment, 3 parts of ultraviolet absorber, 1.5 parts of antioxidant stabilizer, 1.5 parts of dispersant, 6 parts of filler, and 13 parts of solvent.

[0010] As a preferred technical solution of the present invention, the ultraviolet absorber includes one of 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, or 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

[0011] As a preferred technical solution of the present invention, the antioxidant stabilizer is di-tert-butylhydroquinone.

[0012] As a preferred technical solution of the present invention, the dispersant includes one of ethylene-acrylic acid copolymer or oxidized homopolymer.

[0013] As a preferred technical solution of the present invention, the filler is at least one of calcium carbonate, silicon dioxide or titanium dioxide.

[0014] The present invention also provides a method for preparing a high-extensibility and high-rebound TPU color-changing film as described above, comprising the following steps:

[0015] Step S1: Prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0016] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 1-3.5 hours;

[0017] Step 3 S3, preheating the mixed solution A after standing by using a heater, and preheating the mixture A to a temperature of 105-180 ° C. to heat the mixture A to a fluid state, and then standing for a time T2 of 1-5 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 35-70 ° C., the stirring time is 8 min to 15 min, and the stirring speed is 700-1000 r / min;

[0018] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 350-600 mesh and a pressure range of 1.2-2.5 MPa;

[0019] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 120-180°C and the baking time T3 is 3-5 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0020] As a preferred technical solution of the present invention, the standing setting time T1 in step S2 is 2 hours, the preheating temperature in step S3 is 150°C, and the standing time T2 is 2.5 hours, the stirring temperature is 32°C, the stirring time is 10 minutes, and the stirring speed is 800 r / min.

[0021] As a preferred technical solution of the present invention, the filter mesh number of the filter in step S4 is 560 mesh, and the pressure value of the material pressurization is 1.5 MPa.

[0022] As a preferred technical solution of the present invention, the number of times the filtered solution is coated in step S5 is at least 3 times, the baking temperature of the baking chamber is 130° C., and the baking time T3 is 3.5 minutes.

[0023] The present invention relates to a high-extensibility and high-rebound TPU color-changing film and a preparation method thereof, which have the following beneficial effects: the high-extensibility and high-rebound TPU color-changing film of the present invention contains a thermoplastic polyester elastomer with a hardness of 45A-60A on the basis of aliphatic polyurethane, has a combination of multiple high molecular polymers, changes the chemical formula of the substance, can extend under the action of a large external force without breaking, and can make the prepared TPU color-changing film have high extensibility; and by adding polyethylene terephthalate fiber to the prepared ingredients, utilizing its high strength and elastic recovery ability, the TPU color-changing film can also have high resilience.

[0024] The present invention will be further described below in conjunction with specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 One of the images captured for the application of the present invention for a high-extensibility and high-resilience TPU color-changing film (black);

[0026] Figure 2 This is a picture of the effect of the TPU color-changing film obtained in Example 6 of the present invention being applied to a car. DETAILED DESCRIPTION

[0027] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and are not to be construed as limiting the present invention.

[0028] The disclosure below provides many different embodiments or examples for realizing different structures of the present invention. In order to simplify the disclosure of the present invention, the components and settings of specific examples are described below. Of course, they are merely examples and are not intended to limit the present invention. In addition, the present invention may repeat reference numbers and / or reference letters in different examples. Such repetition is for the purpose of simplicity and clarity and does not in itself indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides examples of various specific processes and materials, but those skilled in the art will recognize the application of other processes and / or the use of other materials.

[0029] The present invention provides a high-extensibility and high-rebound TPU color-changing film, which is made according to the weight parts of the following raw materials:

[0030] 30-45 parts of aliphatic polyurethane, 20-40 parts of thermoplastic polyester elastomer with a hardness of 45A-60A, 10-40 parts of polyethylene terephthalate fiber, 4-12 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, 1-5 parts of dispersant, 5-8 parts of filler, and 10-15 parts of solvent.

[0031] In order to obtain the high ductility and high resilience TPU color-changing film of the present invention, the present invention provides 8 embodiments, 3 comparative examples and 1 test example, among which Figure 1 This is a picture taken from the color-changing film obtained in Example 6 of the present invention, in which the application is taken as an example of a car film. Figure 2 The specific experimental process of each of the above embodiments is shown below.

[0032] Example 1

[0033] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0034] 30 parts of aliphatic polyurethane, 20 parts of thermoplastic polyester elastomer with a hardness of 45A, 17 parts of polyethylene terephthalate fiber, 10 parts of pigment, 2 parts of ultraviolet absorber, 5 parts of antioxidant stabilizer, 1 part of dispersant, 5 parts of filler, and 10 parts of solvent.

[0035] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0036] Step 1 S1, prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0037] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 1-3.5 hours;

[0038] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 105 ° C. to heat the mixture A to a fluid state, and then standing for another time T2 of 3 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 35 ° C., the stirring time is 10 minutes, and the stirring speed is 700 r / min;

[0039] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 350 and a pressure range of 1.5 MPa;

[0040] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 120°C and the baking time T3 is 3 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0041] The ultraviolet absorber in Example 1 is 2,4-dihydroxybenzophenone; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant is ethylene-acrylic acid copolymer; and the filler is calcium carbonate.

[0042] Example 2

[0043] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0044] 32 parts of aliphatic polyurethane, 22 parts of thermoplastic polyester elastomer with a hardness of 48A, 14 parts of polyethylene terephthalate fiber, 9 parts of pigment, 2 parts of ultraviolet absorber, 5 parts of antioxidant stabilizer, 1 part of dispersant, 5 parts of filler, and 10 parts of solvent.

[0045] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0046] Step 1 S1, prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0047] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 1-3.5 hours;

[0048] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 110° C. to heat the mixture A to a fluid state, and then standing again for a time T2 of 1-5 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 35° C., the stirring time is 8 minutes, and the stirring speed is 800 r / min;

[0049] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 360 and a pressure range of 1.2 MPa;

[0050] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 110°C and the baking time T3 is 3 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0051] The ultraviolet absorber in Example 2 is 2-hydroxy-4-methoxybenzophenone; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant includes ethylene-acrylic acid copolymer; and the filler is silicon dioxide.

[0052] Example 3

[0053] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0054] 33 parts of aliphatic polyurethane, 20 parts of thermoplastic polyester elastomer with a hardness of 50A, 20 parts of polyethylene terephthalate fiber, 7 parts of pigment, 3 parts of ultraviolet absorber, 1 part of antioxidant stabilizer, 1 part of dispersant, 5 parts of filler, and 12 parts of solvent.

[0055] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0056] Step 1 S1, prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0057] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 1-3.5 hours;

[0058] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 120° C. to heat the mixture A to a fluid state, and then standing again for a time T2 of 2 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 45° C., the stirring time is 11 minutes, and the stirring speed is 750 r / min;

[0059] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 400 and a pressure range of 2 MPa;

[0060] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 145°C and the baking time T3 is 4 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0061] The ultraviolet absorber in Example 3 is 2-hydroxy-4-n-octyloxybenzophenone; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant is an oxidized homopolymer; and the filler is titanium dioxide.

[0062] Example 4

[0063] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0064] 36 parts of aliphatic polyurethane, 25 parts of thermoplastic polyester elastomer with a hardness of 51A, 11 parts of polyethylene terephthalate fiber, 4 parts of pigment, 2.5 parts of ultraviolet absorber, 2.5 parts of antioxidant stabilizer, 2.5 parts of dispersant, 5.5 parts of filler, and 11 parts of solvent.

[0065] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0066] Step S1: Prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0067] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 1-3.5 hours;

[0068] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 150° C. to heat the mixture A to a fluid state, and then standing again for a time T2 of 4 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 50° C., the stirring time is 10 minutes, and the stirring speed is 850 r / min;

[0069] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 600 and a pressure range of 2.5 MPa;

[0070] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 135°C and the baking time T3 is 3.5 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0071] The ultraviolet absorber in Example 4 is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant is an oxidized homopolymer; and the filler is calcium carbonate.

[0072] Example 5

[0073] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0074] 32 parts of aliphatic polyurethane, 32 parts of thermoplastic polyester elastomer with a hardness of 45A, 10 parts of polyethylene terephthalate fiber, 4 parts of pigment, 2 parts of ultraviolet absorber, 1 part of antioxidant stabilizer, 1 part of dispersant, 5 parts of filler, and 12 parts of solvent.

[0075] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0076] Step S1: Prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0077] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container in proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 2 hours;

[0078] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 160° C. to heat the mixture A to a fluid state, and then standing again for 1 hour; polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler are added, and the added ingredients are stirred to obtain a mixed solution B; the stirring temperature is 52° C., the stirring time is 13 minutes, and the stirring speed is 800 r / min;

[0079] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 380 and a pressure range of 2.5 MPa;

[0080] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 180°C and the baking time T3 is 5 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0081] The ultraviolet absorber in Example 5 is 2,4-dihydroxybenzophenone; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant includes ethylene-acrylic acid copolymer; and the filler is calcium carbonate.

[0082] Example 6

[0083] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0084] 32 parts of aliphatic polyurethane, 22 parts of thermoplastic polyester elastomer with a hardness of 55A, 15 parts of polyethylene terephthalate fiber, 6 parts of pigment, 3 parts of ultraviolet absorber, 1.5 parts of antioxidant stabilizer, 1.5 parts of dispersant, 6 parts of filler, and 13 parts of solvent.

[0085] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0086] Step S1: Prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0087] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container in proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 2 hours;

[0088] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 150° C. to heat the mixture A to a fluid state, and then standing again for a time T2 of 1-5 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 32° C., the stirring time is 10 minutes, and the stirring speed is 800 r / min;

[0089] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 560 and a pressure range of 1.5 MPa;

[0090] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 120-130°C and the baking time T3 is 3.5 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0091] The ultraviolet absorber in Example 1 is 2-hydroxy-4-methoxybenzophenone; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant is ethylene-acrylic acid; and the filler is silicon dioxide.

[0092] Example 7

[0093] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0094] 30 parts of aliphatic polyurethane, 34 parts of thermoplastic polyester elastomer with a hardness of 55A, 10 parts of polyethylene terephthalate fiber, 4 parts of pigment, 3 parts of ultraviolet absorber, 1.5 parts of antioxidant stabilizer, 1.5 parts of dispersant, 6 parts of filler, and 10 parts of solvent.

[0095] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0096] Step S1: Prepare the required raw materials: mix the ingredients in the percentage ratio according to the above raw materials;

[0097] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 3 hours;

[0098] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 120° C. to heat the mixture A to a fluid state, and then standing again for 2 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 70° C., the stirring time is 8 minutes, and the stirring speed is 1000 r / min;

[0099] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 600 and a pressure range of 2.0 MPa;

[0100] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 150°C and the baking time T3 is 4 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0101] The ultraviolet absorber in Example 7 is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant is ethylene-acrylic acid copolymer; and the filler is silicon dioxide.

[0102] Example 8

[0103] Raw material ratio - high ductility and high resilience TPU color-changing film, the TPU color-changing film is made according to the weight parts of the following raw materials:

[0104] 30 parts of aliphatic polyurethane, 21 parts of thermoplastic polyester elastomer with a hardness of 60A, 23 parts of polyethylene terephthalate fiber, 4 parts of pigment, 3 parts of ultraviolet absorber, 1 part of antioxidant stabilizer, 1 part of dispersant, 5 parts of filler, and 12 parts of solvent.

[0105] The high-extensibility and high-resilience TPU color-changing film of the present invention is prepared by using the above-mentioned raw materials. The preparation method includes the following steps:

[0106] Step S1, prepare the required raw materials: mix the raw materials according to the percentage ratio of claim 1;

[0107] Step 2 S2: Place the aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container in proportion and stir them evenly with a stirrer to obtain a mixture A, and set the standing time T1 to 3.5 hours;

[0108] Step 3 S3, preheating the mixed solution A after standing still with a heater, and preheating the mixture A to 180° C. to heat the mixture A to a fluid state, and then standing again for a time T2 of 3 hours; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, and filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 70° C., the stirring time is 15 minutes, and the stirring speed is 1000 r / min;

[0109] Step 3 S4: pressurize the mixed solution B in step S3 and filter it with a filter having a mesh size of 600 and a pressure range of 2.5 MPa;

[0110] The third step S5 is to apply the solution filtered in step S4 on the coated paper coated by the coating machine. After coating, it is sent into the baking room for drying through a rubber roller. The baking temperature is 120°C and the baking time T3 is 4 minutes. After cooling and winding, the TPU color-changing film can be obtained.

[0111] The ultraviolet absorber in Example 8 is 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole; the antioxidant stabilizer is di-tert-butylhydroquinone; the dispersant is ethylene-acrylic acid copolymer; and the filler is calcium carbonate.

[0112] Test example

[0113] During the preparation process, no aliphatic polyurethane, thermoplastic polyester elastomer, or polyethylene terephthalate fiber was added; other preparation conditions were the same as those in Example 1.

[0114] Comparative Example 1

[0115] During the preparation of the color-changing film, no aliphatic polyurethane was added; other preparation conditions were the same as those in Example 1.

[0116] Comparative Example 2

[0117] During the preparation of the color-changing film, no thermoplastic polyester elastomer was added; other preparation conditions were the same as those in Example 1.

[0118] Comparative Example 3

[0119] During the preparation of the color-changing film, polyethylene terephthalate fiber was not added; other preparation conditions were the same as those in Example 1.

[0120] It should be noted that the differences among Examples 1-8 of the present application are that the ratios of the raw materials and the processing indicators in the preparation methods are different (such as stirring time, temperature setting value, etc.).

[0121] The TPU color-changing films obtained by the application examples 1-8, test examples and comparative examples 1-3 of the present invention were subjected to project tests; the test items included tensile testing and resilience testing; the standard for the tensile test was based on GB / T16491-1996. When conducting the tensile test, the corresponding standard requirements must be followed to ensure the accuracy and reliability of the test results; the relevant standards stipulate that the displacement and force ratings of the color-changing film sample after tensile fracture are used to calculate the tensile strength and elongation at break (nominal strain at break), which are used as a basis for judging whether the material's tensile strength and elongation at break test items meet the standard requirements; the aforementioned test equipment is a tensile testing machine, which uses a test product produced by Liboshi Instrument Equipment Co., Ltd.

[0122] The tensile test results are shown in Table 1 below.

[0123]

[0124]

[0125] The above-mentioned resilience test adopts the digital pressure gauge method. The test principle is to use a digital pressure gauge to test the color-changing film and calculate the resilience of the color-changing film by observing the changes in the readings. The digital pressure gauge used is a Yuan Hengtong product. The product information is shown in Table 2 below:

[0126]

[0127] The test steps are summarized as follows: ① Use a digital pressure gauge to test each color-changing film to be tested and record the readings; ② Release the test pressure and observe the changes in the readings; ③ Calculate the resilience of the color-changing film based on the changes in the readings. The test results are shown in Table 3 below:

[0128]

[0129]

[0130] From Table 1 above, it can be seen that the tensile strength of the TPU color-changing film embodiments 1-8 of the present invention is distributed above 80 MPa, and the elongation at break of the embodiments 1-8 is greater than or equal to 150%, while that of the comparative examples 1-3 and the test examples is lower; from Table 3 above, it can be seen that the digital display values ​​after rebound in the TPU color-changing film embodiments 1-8 of the present invention are all greater than 7.5 N, while the digital display values ​​after rebound in the comparative examples 1-3 are between 5.0 and 7.0 N, and the digital display value after rebound in the test example is only 1.21 N; combined with Figure 1 and Figure 2It can be seen that the high ductility and resilience performance of Example 6 are the best; therefore, the TPU color-changing film obtained by the present invention contains aliphatic polyurethane and a thermoplastic polyester elastomer with a hardness of 45A-60A, which has a combination of multiple high molecular polymers, changes the chemical formula of the substance, and can extend without breaking under the action of a large external force, so that the prepared TPU color-changing film has high ductility; and polyethylene terephthalate fiber is added to the prepared ingredients, and its high strength and elastic recovery ability are utilized to make the TPU color-changing film also have high resilience.

[0131] Throughout this specification, reference to terms such as "one embodiment," "certain embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples" means that a specific feature, structure, material, or characteristic described in conjunction with the embodiment or example is included in at least one embodiment or example of the present invention. In this specification, illustrative descriptions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0132] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the inventive concept of the present invention, which all fall within the scope of protection of the present invention.

Claims

1. A high-extensibility and high-rebound TPU color-changing film, characterized in that: The TPU color-changing film is made according to the following raw materials in parts by weight: 30-45 parts of aliphatic polyurethane, 20-40 parts of thermoplastic polyester elastomer with a hardness of 45A-60A, 10-40 parts of polyethylene terephthalate fiber, 4-12 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, 1-5 parts of dispersant, 5-8 parts of filler, and 10-15 parts of solvent.

2. A high-extensibility and high-resilience TPU color-changing film as claimed in claim 1, characterized in that: The TPU color-changing layer is calculated based on the weight parts of the following raw materials: 32 parts of aliphatic polyurethane, 22 parts of thermoplastic polyester elastomer with a hardness of 55A, 15 parts of polyethylene terephthalate fiber, 6 parts of pigment, 3 parts of ultraviolet absorber, 1.5 parts of antioxidant stabilizer, 1.5 parts of dispersant, 6 parts of filler, and 13 parts of solvent.

3. The high-extensibility and high-resilience TPU color-changing film according to claim 1, characterized in that: The ultraviolet absorber includes one of 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, and 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

4. The high-elongation and high-resilience TPU color-changing film according to claim 1, characterized in that: The antioxidant stabilizer is di-tert-butylhydroquinone.

5. A high-extensibility and high-resilience TPU color-changing film according to any one of claims 1 to 4, characterized in that: The dispersant includes one of an ethylene-acrylic acid copolymer or an oxidized homopolymer.

6. A high-extensibility and high-resilience TPU color-changing film according to any one of claims 1 to 4, characterized in that: The filler is at least one of calcium carbonate, silicon dioxide or titanium dioxide.

7. A method for preparing a high-extensibility and high-resilience TPU color-changing film according to any one of claims 1 to 6, characterized in that: The following steps are included Step S1, preparing the required raw materials: mixing the raw materials according to claim 1 in percentage proportion; Step 2 S2, placing aliphatic polyurethane, thermoplastic polyester elastomer and solvent into a mixing container according to a proportion and stirring them evenly with a stirrer to obtain a mixture A, and setting the standing time T1 to 1-3.5h; Step 3 S3, preheating the mixed solution A after standing by a heater, and preheating the mixture A to 105-180°C to heat the mixture A to a fluid state, and standing for a time T2 of 1-5h again; adding polyethylene terephthalate fiber, pigment, ultraviolet absorber, antioxidant stabilizer, dispersant, filler, and stirring the added ingredients to obtain a mixed solution B; the stirring temperature is 35-70°C, the stirring time is 8min-15min, and the stirring speed is 700-1000r / min; Step 3 S4, pressurizing the mixed solution B in step S3 and filtering it with a filter, the filter mesh number is 350-600 mesh, and the pressure value range is 1.2-2.5MPa; The third step S5, apply the solution filtered in step S4 on the coated paper coated by the coating machine, and after coating, send it into the baking room for drying through a rubber roller, the baking temperature is 120-180℃, the baking time T3 is 3-5min, and then the TPU color-changing film is obtained after cooling and winding.

8. The preparation method according to claim 7, characterized in that: The setting time T1 for standing in step S2 is 2 hours, the preheating temperature in step S3 is 150° C., the standing time T2 is 2.5 hours, the stirring temperature is 32° C., the stirring time is 10 minutes, and the stirring speed is 800 r / min.

9. The preparation method according to claim 7, characterized in that: In step S4, the filter mesh number of the filter is 560 meshes, and the pressure value of the material pressurization is 1.5 MPa.

10. The preparation method according to claim 7, characterized in that: In step S5, the filtered solution is coated at least three times, the baking temperature of the baking chamber is 130° C., and the baking time T3 is 3.5 min.