Silicone resin heat conduction composition and preparation method thereof

By loading aluminum silicate on the surface of mica and using a combination of multiple thermal fillers, the contradiction between the thermal conductivity improvement of silicone resin thermal conductivity and the lightweighting of equipment is solved, and efficient thermal conductivity improvement and thermal stability enhancement are achieved.

CN118909442APending Publication Date: 2024-11-08JIANGYIN ZHITONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410969872.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

While the existing silicone thermal conductivity increases the thermal conductivity, the equipment increases weight due to the increase in the specific gravity of the thermal filler, which affects the lightweight design and the thermal conductivity improvement is limited.

Method used

By loading aluminum silicate on the mica surface, increasing the specific surface area of ​​mica sheets and contact rate with other thermal fillers, a combination of three thermal fillers, including spherical and smaller particle size fillers, optimize the filling density and improve the silicone resin Thermal conductivity of the heat conduction composition.

Benefits of technology

It achieves the improvement of thermal conductivity of silicone resin thermally conductive materials while ensuring insulation performance, reduce contact thermal resistance, enhance heat resistance and reduce the adverse effects of equipment weight increase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952835890000071
    Figure BDA0004952835890000071
  • Figure BDA0004952835890000081
    Figure BDA0004952835890000081
Patent Text Reader

Abstract

The invention discloses a silicon resin heat conduction composition which comprises the following main components in parts by weight: 100 parts of silicon resin, 30-50 parts of spherical first heat conduction filler with the particle size of 30-80 microns, 45-75 parts of second heat conduction filler with the particle size not greater than 5 microns and 23-40 parts of third heat conduction filler with the particle size of 20-40 microns, the third heat-conducting filler is composite powder formed by loading sodium silicate on the surface of mica. The heat-conducting filler in the silicon resin heat-conducting composition is a combination of three heat-conducting fillers, and aluminum silicate is loaded on the surface of two-dimensional mica, so that the insulating property is ensured, and meanwhile, the aluminum silicate forms a rough structure on the relatively smooth surface of the mica, so that the heat dissipation area of the mica is increased; by optimizing the grading of the heat-conducting fillers with different particle sizes and shapes, the filling compactness of the heat-conducting fillers in the silicon resin is improved, and the heat-conducting property of the silicon resin heat-conducting composition is improved. The invention also discloses a preparation method of the silicon resin heat conduction composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat conduction materials, and in particular to a silicone heat conduction composition and a preparation method thereof. Background Art

[0002] The main function of silicone heat conductive material is to fill between the heating element and the heat sink of electronic parts and accelerate the heat conduction between the heating element and the heat sink to reduce the damage of high temperature to the electronic device chip.

[0003] The main components of insulating silicone thermal conductive materials are silicone resin and insulating thermal conductive fillers. The insulating thermal conductive fillers can be selected from oxides, hydroxides, nitrides, carbides, such as aluminum oxide, zinc oxide, aluminum hydroxide, silicon dioxide, silicon nitride, silicon carbide, etc. On the basis of ensuring the fluidity of silicone thermal conductive materials, the content of thermal conductive fillers is increased, and the thermal conductivity and specific gravity of silicone thermal conductive materials are also increased accordingly. A larger specific gravity leads to an increase in the weight gain of wearable devices or mobile devices, which is not conducive to the lightweighting of the equipment. In addition, further improving the thermal conductivity of silicone thermal conductive materials is also a basic research and development direction of silicone thermal conductive materials. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects existing in the prior art and provide a silicone resin thermal conductive composition, which loads aluminum silicate on the surface of mica to increase the specific surface area of ​​the mica sheet, avoid and increase the probability of direct contact and effective heat transfer between the mica sheet and other thermal conductive fillers, and improve the thermal conductivity of the silicone resin thermal conductive composition.

[0005] In order to achieve the above technical effects, the technical solution of the present invention is: a silicone resin heat conductive composition, which mainly comprises, by weight, 100 parts of silicone resin, 30 to 50 parts of a spherical first heat conductive filler with a particle size of 30 to 80 μm, 45 to 75 parts of a second heat conductive filler with a particle size of no more than 5 μm, and 23 to 40 parts of a third heat conductive filler with a particle size of 20 to 40 μm;

[0006] The third thermally conductive filler is a composite powder with sodium silicate loaded on the surface of mica.

[0007] Further, the main components of the silicone resin heat conductive composition include, by weight: 100 parts of silicone resin, 36-42 parts of a spherical first heat conductive filler having a particle size of 30-80 μm, 52-63 parts of a second heat conductive filler having a particle size of no more than 5 μm, and 28-33 parts of a third heat conductive filler having a particle size of 20-40 μm;

[0008] The preferred technical solution is that the mass ratio of mica to aluminum silicate in the mica composite powder is 1:(0.65-1). The mass of aluminum silicate is the theoretical value obtained by the reaction of sodium silicate and aluminum sulfate. The mass ratio of mica to aluminum silicate in the mica composite powder can be selected as 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1 point values ​​and an interval with two of the points as the maximum and minimum values.

[0009] A preferred technical solution is that the aspect ratio of mica in the mica composite powder is 30-60, and further, the aspect ratio of mica is 30-45.

[0010] A preferred technical solution is that the first thermally conductive filler is silicon dioxide or silicon nitride, and / or the second thermally conductive filler is aluminum oxide or zinc oxide.

[0011] The second object of the present invention is to provide a method for preparing a silicone resin thermal conductive composition, based on the above silicone resin thermal conductive composition, comprising the steps of preparing the composite powder:

[0012] S01: ultrasonically dispersing mica powder in water to obtain a mica dispersion, and heating the dispersion to 60-80° C.;

[0013] S02: Add aluminum sulfate solution and sodium silicate solution to the mica dispersion at a molar ratio of aluminum to silicon of 1:1, keep warm for 0.5 to 2 hours, centrifuge, wash, dry, calcine and cool in sequence to obtain a composite powder.

[0014] The preferred technical solution is that the calcination atmosphere in S02 is nitrogen, the calcination temperature is 500-600°C, and the calcination time is 0.5-2h. The calcination temperature can be specifically selected from 500°C, 520°C, 550°C, 580°C, 600°C, and an interval with two of the points as the maximum and minimum values, and is further preferably 550-600°C;

[0015] The preferred technical solution is that after S02, the following steps are included:

[0016] S03: premixing the composite powder with the second thermally conductive filler, and then mixing with the first thermally conductive filler to obtain a thermally conductive filler mixed powder;

[0017] S04: Evenly mix the thermal conductive filler mixed powder and the silicone resin to obtain a silicone resin thermal conductive composition.

[0018] The preferred technical solution is that S01 further includes: adding ammonia water to the mica dispersion to adjust the pH value of the mica dispersion to 10.5 to 12. Furthermore, the pH value of the mica dispersion can be selected from 10.5, 11, 11.5, 12 points and an interval with two of the points as the maximum and minimum values.

[0019] The preferred technical solution is that the mass concentration of the sodium silicate solution in S02 is 3% to 10%, the dripping speed of sodium silicate is 0.5 to 2 ml / min, and the solid-liquid ratio of mica powder to water is 1: (12 to 20). Furthermore, the mass concentration of the sodium silicate solution in S02 is 4% to 7%, the dripping speed of sodium silicate is 1 to 2 ml / min, and the solid-liquid ratio of mica powder to water is 1: (12 to 17). The solid-liquid ratio of mica powder to water refers to the mass ratio.

[0020] The preferred technical solution is that a new ball mill is used for premixing S03, and the ball milling process is: negative pressure nitrogen atmosphere, ball mill speed 100-200 rpm, ball to material ratio (12-20): 1, ball milling time 0.5-2h. Further, the ball to material ratio is (14-17): 1.

[0021] The advantages and beneficial effects of the present invention are:

[0022] The heat-conducting filler in the silicone resin heat-conducting composition adopts a combination of three heat-conducting fillers, wherein aluminum silicate is loaded on the surface of the two-dimensional mica to ensure the insulation performance while the aluminum silicate forms a rough structure on the relatively smooth mica surface, which is beneficial to increase the heat dissipation area of ​​the mica;

[0023] The rough structure of aluminum silicate is also conducive to increasing the contact probability with the second thermal conductive filler with a smaller particle size and the first thermal conductive filler with a larger particle size, thereby reducing the contact thermal resistance;

[0024] By optimizing the gradation of thermally conductive fillers with different particle sizes and shapes, the filling density of the thermally conductive fillers in the silicone resin is improved, and the thermal conductivity of the silicone resin thermal conductive composition is improved. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.

[0026] Silicone

[0027] Silicone resin is used as a dispersion base material for thermally conductive powders. It is a cross-linked semi-inorganic polymer with silicon-oxygen-silicon as the main chain and organic groups connected to silicon atoms. Thermal conductive compositions based on silicone resin are mainly used for bonding metals, glass, and ceramics. It is understood that the silicone resin thermal conductive composition also includes known additives such as a curing agent for accelerating curing, a retarder for delaying curing, and an inhibitor.

[0028] Second thermally conductive filler

[0029] The second thermally conductive filler has a medium particle size and is filled between the first thermally conductive filler and the third thermally conductive filler. The powder shape of the second thermally conductive filler can be spherical, quasi-spherical, rod-shaped, or flake-shaped, preferably at least one of spherical, quasi-spherical, and rod-shaped.

[0030] Particle size

[0031] The particle sizes of the first thermally conductive filler, the second thermally conductive filler and the third thermally conductive filler are all average particle sizes D50.

[0032] Silicone resin: Dow Corning two-component silicone potting compound Q3-6575;

[0033] Sodium silicate: chemically pure;

[0034] Aluminum sulfate: chemically pure;

[0035] Ammonia: industrial grade;

[0036] Silica, spherical, D50 is 50 μm;

[0037] Alumina, spherical, D50 is 3μm;

[0038] Muscovite, diameter-to-thickness ratio 30-40, D50 30μm;

[0039] Aluminum silicate, D50 is 7 μm;

[0040] Example

[0041] The method for preparing the silicone heat conductive composition comprises the following steps:

[0042] S01: ultrasonically dispersing mica powder in water to obtain a mica dispersion, wherein the solid-liquid ratio of mica powder to water is 1:15, and heating to 75°C;

[0043] S02: Prepare 10% aluminum sulfate solution and 5% sodium silicate solution by mass concentration, measure aluminum sulfate solution and sodium silicate solution according to the mass ratio of mica to theoretically generated aluminum silicate of 1:0.85, and simultaneously add aluminum sulfate solution and sodium silicate solution to the mica dispersion according to the aluminum-silicon molar ratio of 1:1, and the dropping speed of sodium silicate is 1 ml / min. After the addition is completed, keep the reaction warm for 1.5 hours, centrifuge to remove the supernatant, wash with deionized water (to remove sodium ions in the powder), and dry;

[0044] calcining the dried powder in a nitrogen atmosphere at a temperature of 570°C for 1 hour, and cooling to obtain a composite powder;

[0045] S03: mixing the first thermally conductive filler silica, the second thermally conductive filler alumina and the third thermally conductive filler composite powder in a V-type mixer for 1 hour;

[0046] S04: Mix the thermal conductive filler mixed powder and the silicone resin according to a weight fraction ratio, and mechanically stir at 200 r / min for 3 hours to obtain a silicone resin thermal conductive composition.

[0047] Comparative Example 1

[0048] Mica was used to replace the composite powder in the embodiment, and the first thermal conductive filler silicon dioxide, the second thermal conductive filler aluminum oxide and mica were mixed in a V-type mixer for 1 hour;

[0049] The heat-conductive filler mixed powder and the silicone resin are uniformly mixed in proportion by weight to obtain a silicone resin heat-conductive composition.

[0050] Comparative Example 2

[0051] Mica and aluminum silicate replace the composite powder in the embodiment, the mass ratio of mica and aluminum silicate is copper composite powder, the first thermal conductive filler silica, the second thermal conductive filler alumina, mica, and aluminum silicate are mixed in a V-type mixer for 1 hour, and then the silicone resin thermal conductive composition is prepared.

[0052] The compositions of the silicone resin heat conduction compositions of Examples 1-4 and Comparative Examples 1-2 are shown in the following table:

[0053] Silicone The first thermally conductive filler Second thermally conductive filler The third thermal conductive filler Mica Aluminum silicate Example 1 100 copies 40 servings 65 servings 25 servings —— —— Example 2 100 copies 43 servings 52 servings 35 servings —— —— Example 3 100 copies 40 servings 60 servings 30 servings —— —— Example 4 100 copies 37 servings 60 servings 33 servings —— —— Comparative Example 1 100 copies 40 servings 60 servings —— 30 servings Comparative Example 2 100 copies 40 servings 60 servings —— 16.2 servings 13.8 servings

[0054] Thermal conductivity test of silicone thermal conductive composition:

[0055] The silicone resin heat conductive composition obtained from S04 was coated on the surface of the substrate and cured at 70° C. for 40 minutes to prepare a 2 mm thick heat conductive sheet, which was then cut into 5*5 mm square gaskets.

[0056] 1. Test the room temperature thermal conductivity of the square gasket;

[0057] 2. Heat resistance stability: place the gasket in an air environment at 200°C for aging for 200 hours, and test the weight reduction rate before and after aging.

[0058] Weight reduction rate = (gasket mass before aging - gasket mass after aging) / mass before aging The test results of the gasket thermal conductivity performance of Examples 1-4 and Comparative Examples 1-2 are shown in the following table:

[0059] Thermal conductivity (W / M·k) Weight reduction rate (%) Example 1 1.722 1.30 Example 2 1.698 1.33 Example 3 1.734 1.26 Example 4 1.727 1.30 Comparative Example 1 1.563 1.80 Comparative Example 2 1.588 1.73

[0060] Comparative Example 1 and Comparative Example 2: The addition of aluminum silicate to the silicone resin thermal conductive composition helps to improve the thermal conductivity;

[0061] Example 3 and Comparative Example 1: Aluminum silicate loaded on the surface of mica is beneficial to improving the thermal conductivity. The possible reasons are: first, the aluminum silicate powder added in Comparative Example 2 has pores inside and the interface thermal resistance is large; second, the aluminum silicate loaded on the surface of mica in Example 3 is tightly attached, and the fine aluminum silicate particles increase the specific surface area of ​​mica, and also increase the probability of close contact between the third thermally conductive filler and other thermally conductive fillers, especially the second thermally conductive filler, thereby optimizing the thermal conductivity effect.

[0062] Examples 1-4: Based on the same silicone resin, the gradation of the thermally conductive filler is closely related to the thermal conductivity and weight reduction rate of the gasket; in comparison, the gradation of the thermally conductive filler in Examples 3 and 4 is better.

[0063] Examples 1-4 and Comparative Examples 1 and 2: The higher the thermal conductivity of the gasket, the smaller the weight loss after aging treatment, and the better the heat resistance stability.

[0064] Example 5-11

[0065] Embodiment 5-11 is based on embodiment 3, and the difference is:

[0066] S01 of Example 5: ultrasonically dispersing mica powder in water to obtain a mica dispersion, wherein the solid-liquid ratio of mica powder to water is 1:15, adding ammonia water to the mica dispersion, adjusting the pH value to 11, and then heating the mica dispersion to 75° C.;

[0067] S01 of Example 6: ultrasonically dispersing mica powder in water to obtain a mica dispersion, wherein the solid-liquid ratio of mica powder to water is 1:15, adding ammonia water to the mica dispersion, adjusting the pH value to 9, and then heating the mica dispersion to 75° C.;

[0068] S02 of Example 7: Prepare 10% aluminum sulfate solution and 5% sodium silicate solution with a mass concentration, measure the aluminum sulfate solution and the sodium silicate solution according to the mass ratio of mica to theoretically generated aluminum silicate of 1:0.85, and simultaneously add the aluminum sulfate solution and the sodium silicate solution to the mica dispersion at a molar ratio of aluminum to silicon of 1:1, with the dropping speed of sodium silicate being 3.5 ml / min. After the dropwise addition is completed, keep the reaction warm for 1.5 hours, centrifuge to remove the supernatant, wash with deionized water, and dry;

[0069] S02 of Example 8: Prepare 10% aluminum sulfate solution and 5% sodium silicate solution by mass concentration, measure the aluminum sulfate solution and the sodium silicate solution according to the mass ratio of mica to theoretically generated aluminum silicate of 1:0.5, and simultaneously add the aluminum sulfate solution and the sodium silicate solution to the mica dispersion at an aluminum-silicon molar ratio of 1:1, with the sodium silicate being added at a rate of 1 ml / min. After the addition is completed, keep the mixture warm for 1.5 hours, remove the supernatant by centrifugation, wash with deionized water, and dry;

[0070] S02 of Example 9: Prepare 10% aluminum sulfate solution and 5% sodium silicate solution with a mass concentration, measure the aluminum sulfate solution and the sodium silicate solution according to the mass ratio of mica to theoretically generated aluminum silicate of 1:1.2, and simultaneously add the aluminum sulfate solution and the sodium silicate solution to the mica dispersion according to the aluminum-silicon molar ratio of 1:1, the sodium silicate is added at a rate of 1 ml / min, and after the addition is completed, the reaction is kept warm for 1.5 hours, the supernatant is removed by centrifugation, the solution is washed with deionized water, and the solution is dried;

[0071] S03 of Example 10 includes two steps:

[0072] S031: The composite powder and the second thermally conductive filler are premixed in a planetary ball mill. The ball milling process is as follows: 0.9 atm nitrogen atmosphere, ball mill speed of 200 rpm, zirconium ball diameter of 3 mm, ball-to-material ratio of 15:1, ball milling time of 40 min, to obtain a premixed powder of the third thermally conductive filler and the second thermally conductive filler;

[0073] S032: Mix the first thermally conductive filler silica and the premixed powder in a V-type mixer for 1 hour.

[0074] S02 of Example 11: calcining the dried powder in a nitrogen atmosphere at a temperature of 400° C. for 1 h, and cooling to obtain a composite powder;

[0075] The test results of the thermal conductivity performance of the gaskets of Examples 5-10 are shown in the following table:

[0076]

[0077]

[0078] Example 3 and Examples 5 and 6: The appropriate pH value of the mica dispersion is more conducive to the adhesion of aluminum silicate to the mica surface, so that the aluminum silicate is evenly distributed on the mica surface, and the specific surface area of ​​the composite powder is further increased.

[0079] Example 3 and Example 7: The sodium silicate droplet acceleration is too fast, and the aluminum silicate in the mica dispersion aggregates with each other to form an aluminum silicate precipitate, the amount of adhesion on the mica surface is reduced, the increase in the specific surface area of ​​the composite powder is reduced, and the thermal conductivity of the gasket is lower than that of Example 3.

[0080] Example 3 and Examples 8 and 9: if the total amount of aluminum silicate on the mica surface decreases, the increase in the specific surface area of ​​the composite powder will also decrease accordingly, and the thermal conductivity of the gasket in Example 8 is lower than that in Example 3; conversely, if the total amount of aluminum silicate on the mica surface is too large, aluminum silicate will be deposited on the mica surface to form interlayer pores, and the thermal conductivity of the composite powder will decrease. The thermal conductivity of the gasket in Example 9 is further lower than that in Example 8.

[0081] Embodiment 3 and Embodiment 10: The composite powder is pre-mixed with the second thermally conductive filler with a smaller particle size by ball milling, so as to increase the probability of the composite powder adhering to the second thermally conductive filler, and the composite powder and the second thermally conductive filler are mixed evenly, and the thermal conductivity of the gasket is further improved.

[0082] Example 3 and Example 11: Compared with the calcination temperature of 400°C, the calcination temperature of 570°C can remove part of the crystalline water of mica, making the lattice more compact and stable, and the composite powder does not undergo obvious volume changes, which is beneficial to improving the overall thermal conductivity of the composite powder and the gasket.

[0083] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A silicone resin heat conductive composition, characterized in that: The main components include, by weight, 100 parts of silicone resin, 30 to 50 parts of a spherical first thermally conductive filler with a particle size of 30 to 80 μm, 45 to 75 parts of a second thermally conductive filler with a particle size not greater than 5 μm, and 23 to 40 parts of a third thermally conductive filler with a particle size of 20 to 40 μm. The third thermally conductive filler is a composite powder of mica with sodium silicate loaded on the surface.

2. The silicone resin heat conductive composition according to claim 1, wherein The mass ratio of mica to aluminum silicate in the mica composite powder is 1:(0.65-1).

3. The silicone resin heat conductive composition according to claim 1, wherein The aspect ratio of the mica in the mica composite powder is 30-60.

4. The silicone resin heat conductive composition according to claim 1, wherein The first thermally conductive filler is silicon dioxide or silicon nitride, and / or the second thermally conductive filler is aluminum oxide or zinc oxide.

5. A method for preparing a silicone resin heat conductive composition, characterized in that: The silicone resin heat conductive composition according to any one of claims 1 to 4, comprising the steps of preparing the composite powder: S01: ultrasonically dispersing mica powder in water to obtain a mica dispersion, and heating the dispersion to 60-80°C; S02: Aluminum sulfate solution and sodium silicate solution are added dropwise to the mica dispersion at a molar ratio of aluminum to silicon of 1:1, and the mixture is kept warm for 0.5 to 2 hours. The mixture is centrifuged, washed, dried, calcined, and cooled in sequence to obtain a composite powder.

6. The method for preparing the silicone resin heat conductive composition according to claim 5, wherein: The calcination atmosphere in S02 is nitrogen, the calcination temperature is 500-600°C, and the calcination time is 0.5-2h.

7. The method for preparing the silicone resin heat conductive composition according to claim 5, wherein: S02 includes the following steps: S03: pre-mixing the composite powder with the second thermally conductive filler, and then mixing it with the first thermally conductive filler to obtain a thermally conductive filler mixed powder; S04: Evenly mix the thermal conductive filler mixed powder and the silicone resin to obtain a silicone resin thermal conductive composition.

8. The method for preparing the silicone resin heat conductive composition according to claim 5, wherein: S01 further includes: adding ammonia water dropwise to the mica dispersion to adjust the pH value of the mica dispersion to 10.5-12.

9. The method for preparing the silicone resin heat conductive composition according to claim 5, wherein: The mass concentration of the sodium silicate solution in S02 is 3% to 10%, the dropping speed of sodium silicate is 0.5 to 2 ml / min, and the solid-liquid ratio of mica powder to water is 1: (12 to 20).

10. The method for preparing the silicone resin heat conductive composition according to claim 7, wherein: S03 pre-mixing adopts a new type of ball mill, and the ball milling process is: negative pressure nitrogen atmosphere, ball mill speed 100-200 rpm, ball-to-material ratio (12-20): 1, and ball milling time 0.5-2h.