High-flame-retardant silica gel impregnated material for piezoresistor and preparation method of high-flame-retardant silica gel impregnated material

By using the formulation of high flame retardant silicone impregnant in the varistor, including the combination of inorganic and organic flame retardants and ceramic additives, the fire problem of varistors in the prior art in high temperature environment is solved, and the fire problem of varistors in high temperature environment is achieved. There is no open flame effect after overpressure, and the flexibility and temperature cycling performance are improved.

CN118909450APending Publication Date: 2024-11-08TIANJIN CITY KAIHUA INSULATION MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411104965.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing varistors are prone to aging or cause fires when overvoltage is in high temperature environments, and existing flame retardant materials cannot meet the requirements of overvoltage and no open flames.

Method used

The formulation of high flame retardant silicone impregnants, including the combination of inorganic flame retardants, silicone flame retardants and ceramic additives, improve the flame retardant performance through specific process treatment, and prepare to be able to continuously power on at least after overvoltage. Silicone material without open flame for 1 minute.

Benefits of technology

The flame retardant effect without open flame after the varistor is overvoltage, provides better flexibility and temperature cycling performance, is suitable for larger electronic products, and simplifies the preparation process for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of materials, in particular to a high-flame-retardant silica gel impregnated material for a piezoresistor and a preparation method of the high-flame-retardant silica gel impregnated material. The high-flame-retardant silica gel impregnating material for the piezoresistor comprises the following components: vinyl silicone oil, reinforcing resin, an inorganic flame retardant, a ceramization auxiliary agent, an organic silicon flame retardant, a tackifier, a catalyst, a cross-linking agent, an inhibitor, a heat stabilizer and a solvent. In the components, the inorganic flame retardant, the organic silicon flame retardant and the ceramic auxiliary agent are compounded for use, so that the flame retardant property is good, and the requirement that the whole process is free of open fire after the piezoresistor is subjected to overvoltage (no fuse) and then is continuously electrified for at least 1 minute can be met. The preparation method of the high-flame-retardant silica gel impregnated material for the piezoresistor, provided by the invention, is simple in preparation process and suitable for industrial production, and conditions are easy to control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a highly flame-retardant silicone impregnating material for a varistor and a preparation method thereof. Background Art

[0002] A varistor is a resistor device with nonlinear volt-ampere characteristics. It is mainly used to clamp voltage when the circuit is subjected to overvoltage and absorb excess current to protect sensitive devices. Due to the specific application scenarios of varistors, varistors are exposed to high temperature environments for a long time. When the varistor ages or experiences electrical breakdown due to instantaneous overvoltage, the current is too large, causing the insulating material to catch fire, causing a fire.

[0003] CN116844801A discloses an explosion-proof and flame-proof varistor. Although the flame-retardant effect of the inner coating silicone resin is good, the flame-retardant of the outer coating epoxy material cannot meet the requirements of overvoltage (no fuse) and no open flame. CN116063854A discloses a two-component flame-retardant ceramic silica gel and its preparation method and application: the flame-retardant effect of the flame-retardant ceramic silica gel disclosed in this patent cannot meet the requirements of overpressure (no fuse) and no open flame.

[0004] CN114410120A discloses a single-component flame-retardant silicone impregnating material, method and application for varistor. The flame-retardant effect of the flame retardant for varistor disclosed in this patent cannot meet the requirement of no open flame under overvoltage (no fuse). Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the related art. To this end, the first object of the present invention is to provide a highly flame-retardant silicone impregnating material for a varistor; the second object of the present invention is to provide a preparation method of a highly flame-retardant silicone impregnating material for a varistor.

[0006] In order to achieve the first purpose, the technical solution adopted by the present invention is: A highly flame-retardant silicone impregnating material for a varistor, the components and mass fractions of which are as follows: Vinyl silicone oil, 15 to 40 parts; Reinforcing resin, 0-10 parts; Inorganic flame retardant, 20 to 40 parts; Ceramizing agent, 30 to 60 parts; Silicone flame retardant, 1 to 10 parts; Thickener, 0.5 to 4 parts; Catalyst, 0.1 to 0.3 parts; Cross-linking agent, 1 to 5 parts; Inhibitor, 0.1 to 0.5 parts; Heat stabilizer, 1 to 5 parts; Solvent: 10 to 20 parts.

[0007] Preferably, the vinyl silicone oil is a single viscosity vinyl silicone oil or is compounded from vinyl silicone oils of different viscosities; Wherein, when the vinyl silicone oil is compounded with vinyl silicone oils of different viscosities, the viscosity of the vinyl silicone oil is ≥1000 mPa·s.

[0008] Preferably, the vinyl silicone oil is vinyl polysiloxane, and the vinyl polysiloxane includes at least one of vinyl-terminated polydimethylsiloxane, vinyl-terminated polymethylphenylsiloxane and vinyl-terminated boron-containing silicone oil.

[0009] Preferably, the inhibitor is at least one of diallyl maleate, diethyl fumarate, ethynyl cyclohexanol and 3,7,11-trimethyldodecyn-3-ol.

[0010] Preferably, the reinforcing resin is MQ silicone resin, and the MQ silicone resin is any one of methyl vinyl MQ silicone resin and methyl phenyl vinyl MQ silicone resin; Among them, the ratio of M to Q is 0.6 to 1.2, and the vinyl mass content is 2% to 3.5%.

[0011] Preferably, the cross-linking agent side hydrogen-containing silicone oil or the end side hydrogen-containing silicone oil has a viscosity of 55 mPa·s to 120 mPa·s and a hydrogen content of 0.30% to 1.25%.

[0012] Preferably, the tackifier is a liquid tackifier with a viscosity of 10 mPa·s to 200 mPa·s, and the tackifier structure contains at least two groups selected from epoxy, acyloxy, carbonyl, hydroxyl, silanol, silane and alkoxy.

[0013] Preferably, the inorganic flame retardant is compounded by a first flame retardant and a second flame retardant, the first flame retardant is at least one of aluminum hydroxide and magnesium hydroxide, and the second flame retardant is at least one of basic magnesium carbonate, basic zinc carbonate and zinc hydroxystannate; Wherein, the mass ratio of the second flame retardant to the inorganic flame retardant is 1 / 5 to 1 / 3.

[0014] Preferably, the inorganic flame retardant is used after being treated with a first coupling agent, and the treatment process is as follows: Adding an inorganic flame retardant to a mixing device, spraying the first coupling agent / ethanol solution into the mixing device when mixing the inorganic flame retardant, and baking at 100° C. to 180° C. for 1 h to 3 h after mixing; Wherein, the mass ratio of the first coupling agent to ethanol is 1:20 to 1:10; The first coupling agent is at least one of KH560, KH570, A171 and A172.

[0015] Preferably, the ceramicizing aid comprises at least three of mica powder, wollastonite, silica powder and glass powder; The glass powder has a melting point of 800°C to 1300°C, a particle size of 325 mesh to 500 mesh, and an aspect ratio of 10:1 to 20:1; The particle size of the mica powder is 325 mesh to 800 mesh; The wollastonite has a particle size of 325 mesh to 1250 mesh and an aspect ratio of 10:1 to 20:1; The particle size of the silicon micropowder is 400-1000 meshes.

[0016] Preferably, the silicon micropowder contains spherical silicon micropowder.

[0017] Preferably, the ceramicizing agent is used after being treated with a second coupling agent, and the treatment process is as follows: Add a ceramicizing agent to a mixing device, spray a second coupling agent / ethanol solution into the mixing device while mixing the ceramicizing agent, and bake at 100° C. to 180° C. for 1 h to 3 h after mixing; Wherein, the mass ratio of the first coupling agent to ethanol is 1:20 to 1:10; The second coupling agent is at least one of KH560, KH570, A171 and A172.

[0018] Preferably, the organosilicon flame retardant comprises cage-type silsesquioxane and ladder-type polysilsesquioxane; Wherein, the cage-type silsesquioxane includes at least one of a glycidyloxy group, a methacryloxy group, an octaphenyl group, an octaisobutyl group, an octavinyl group, an octaoctyl group, an octadodecyl group, an octaepoxycyclohexylethyl group and an acryloxypropyl group; The ladder silsesquioxane includes at least one of phenyl ladder polysilsesquioxane, methacryloxypropyl ladder polysilsesquioxane, glycidyl ether epoxy ladder polysilsesquioxane, and 2-(3,4-epoxyhexyl)ethyl ladder polysilsesquioxane.

[0019] Preferably, the thermal stabilizer comprises at least one of iron oxide and cerium oxide.

[0020] Preferably, the catalyst comprises at least one of chloroplatinic acid, a platinum-methylvinylsiloxane coordination complex and a platinum-alkynyl complex.

[0021] Preferably, the solvent comprises at least one of xylene, toluene and cyclohexane.

[0022] In order to achieve the second purpose, the technical solution adopted by the present invention is: A method for preparing a highly flame-retardant silicone impregnating material for a varistor, which is used to prepare the highly flame-retardant silicone impregnating material for a varistor as described in any one of the above items, comprises the following steps: S100, weighing each component according to the mass fraction of the formula, adding them into a high-speed disperser, and dispersing for 60 minutes to 90 minutes to obtain a first mixture; S200, adding a crosslinking agent into a high-speed disperser containing the first mixture, stirring for 10 to 15 minutes to obtain a second mixture; S300, performing vacuum degassing treatment on the obtained second mixture to obtain a highly flame-retardant silicone impregnating material for a varistor.

[0023] The above one or more technical solutions in the embodiments of the present invention have at least one of the following technical effects: The invention provides a highly flame-retardant silicone impregnating material for a varistor. In its formula, an inorganic flame retardant, an organic silicon flame retardant and a ceramic additive are used in combination to obtain a varistor with good flame retardancy, which can meet the requirement that the varistor can be continuously powered on for at least 1 minute after being over-voltaged (without a fuse) and without open flames during the whole process. Compared with thermosetting silicone resin encapsulating materials with good flame retardancy, the high flame retardant silicone impregnating material for varistor provided by the present invention is a silicone material with better flexibility. For electronic products of larger sizes, it has better temperature cycling performance and will not crack after 1000 cycles.

[0024] The invention provides a method for preparing a highly flame-retardant silicone impregnating material for a varistor, which has a simple preparation process, easy-to-control conditions and is suitable for industrial production.

[0025] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The following embodiments are used to illustrate the present invention, but cannot be used to limit the scope of the present invention.

[0027] A highly flame-retardant silicone impregnating material for a varistor, the components and mass fractions of which are as follows: Vinyl silicone oil, 15 to 40 parts; Reinforcing resin, 0-10 parts; Inorganic flame retardant, 20 to 40 parts; Ceramizing agent, 30 to 60 parts; Silicone flame retardant, 1 to 10 parts; Thickener, 0.5 to 4 parts; Catalyst, 0.1 to 0.3 parts; Cross-linking agent, 1 to 5 parts; Inhibitor, 0.1 to 0.5 parts; Heat stabilizer, 1 to 5 parts; Solvent: 10 to 20 parts.

[0028] Silicone itself is not easy to ignite, has a low heat release rate and slow combustion speed during combustion, and the -Si-O bond on the main chain can be transformed into a continuous, insulating, anti-oxidation network structure. The oxygen index is higher than that of polymers with carbon as the main chain, there is no dripping phenomenon, and no toxic gas is produced during combustion, which makes it a good flame retardant material. This patent uses vinyl silicone oil as the base material. First, there is no small molecule precipitation in the addition type silicone reaction, and second, the platinum catalyst used in it has a certain effect on flame retardancy.

[0029] The vinyl silicone oil in the formula composition of the present invention can be one or more of vinyl polysiloxane, including vinyl-terminated polydimethylsiloxane, vinyl-terminated polymethylphenylsiloxane and vinyl-terminated boron-containing silicone oil; when a plurality of vinyl silicone oils with different viscosities are compounded, in order to apply the process and ensure the process performance, the viscosity of the low-viscosity vinyl silicone oil should be ≥1000mPa·s, and in order to obtain good flame retardant properties, vinyl-terminated polymethylphenylsiloxane and vinyl-terminated boron-containing silicone oil are preferably used.

[0030] The inhibitor in the formulation of the present invention may be a conventional inhibitor in the prior art, preferably at least one of diallyl maleate, diethyl fumarate, ethynyl cyclohexanol and 3,7,11-trimethyldodecyn-3-ol.

[0031] The reinforcing resin in the formula composition of the present invention is preferably MQ silicone resin, and the MQ silicone resin can be any one of methyl vinyl MQ silicone resin and methyl phenyl vinyl MQ silicone resin; MQ silicone resin is a kind of silicone resin composed of monofunctional Si-O units and tetrafunctional Si-O units.

[0032] The crosslinking agent in the formula composition of the present invention is preferably a side hydrogen-containing silicone oil or a terminal side hydrogen-containing silicone oil, with a viscosity of 55 mPa·s to 120 mPa·s and a hydrogen content of 0.30% to 1.25%.

[0033] The tackifier in the formulation of the present invention is preferably a liquid tackifier with a viscosity of 10 mPa·s to 200 mPa·s. The tackifier structure contains at least two groups selected from epoxy, acyloxy, carbonyl, hydroxyl, silanol, silane and alkoxy.

[0034] The inorganic flame retardant with a lower initial decomposition temperature is used in the formula composition of the present invention, and the inorganic flame retardant improves the flame retardant performance. The inorganic flame retardant is compounded by a first flame retardant and a second flame retardant, the first flame retardant is at least one of aluminum hydroxide and magnesium hydroxide, the first flame retardant has a high initial decomposition temperature, decomposition absorbs a large amount of heat, reduces the temperature of the material, releases water vapor, dilutes the combustible gas decomposed by organic matter in the coating during overpressure, and improves the flame retardant performance; the second flame retardant is at least one of basic magnesium carbonate, basic zinc carbonate and zinc hydroxystannate, the second flame retardant has a low initial decomposition temperature, and a small amount of addition can better block or extinguish the initial spark or flame when the varistor is over-voltage broken down.

[0035] The first flame retardant and the second flame retardant are used in combination, and the mass ratio of the second flame retardant to the inorganic flame retardant is 1 / 5 to 1 / 3.

[0036] Preferably, the inorganic flame retardant is used after being treated with a first coupling agent, and the treatment process is as follows: Adding an inorganic flame retardant to a high-speed mixing device, spraying the first coupling agent / ethanol solution into the high-speed mixing device when mixing the inorganic flame retardant, and baking at 100° C. to 180° C. for 1 h to 3 h after mixing; Wherein, the mass ratio of the first coupling agent to the ethanol solution is 1:20 to 1:10; The first coupling agent is at least one of KH560, KH570, A171 and A172.

[0037] The ceramicizing additives in the formula of the present invention include at least three of mica powder, wollastonite, silica powder and glass powder; the needle-shaped wollastonite can significantly improve the thermal stability of silica gel, reduce the heat release rate, and improve the dimensional stability; the flaky structure of the mica powder has a heat-insulating effect, and at the same time adsorbs the silicone rubber molecular chain to improve the stability; the mica has a maximum ignition time and a minimum heat release rate, and forms a high-strength material after burning; the glass powder has a melting point of 800°C to 1300°C and a moderate softening temperature, and after softening, it can better form a eutectic with the mica powder or wollastonite, fill the pores, slow down the overflow of combustible gas, and improve the flame retardant performance.

[0038] The silicon micropowder is preferably spherical silicon micropowder or a mixture of ordinary silicon micropowder and spherical silicon micropowder, wherein the purpose of adding the spherical filler is to improve the process performance.

[0039] Among them, the particle size of the glass powder is 325 mesh to 500 mesh, and the aspect ratio is 10:1 to 20:1; the particle size of the mica powder is 325 mesh to 800 mesh; the particle size of the wollastonite is 325 mesh to 1250 mesh, and the aspect ratio is 10:1 to 20:1; the particle size of the silicon micropowder is 400 mesh to 1000 mesh.

[0040] Preferably, the ceramicizing agent is used after being treated with a second coupling agent, and the treatment process is as follows: Adding a ceramicizing agent to a high-speed mixing device, spraying a second coupling agent / ethanol solution into the ceramicizing agent when the high-speed mixing device is mixing the ceramicizing agent, and baking at 100° C. to 180° C. for 1 to 3 hours after mixing; Wherein, the mass ratio of the second coupling agent to ethanol is 1:20 to 1:10; The second coupling agent is at least one of KH560, KH570, A171 and A172.

[0041] The organosilicon flame retardant in the formula of the present invention includes cage silsesquioxane and ladder polysilsesquioxane; the cage silsesquioxane and ladder polysilsesquioxane in the organosilicon flame retardant will form a dense silicon oxide film at high temperature, which effectively blocks oxygen and heat from being transferred to the inside of the polymer, thereby improving the flame retardant performance of the polymer material.

[0042] Wherein, the cage-type silsesquioxane includes at least one of a glycidyloxy group, a methacryloxy group, an octaphenyl group, an octaisobutyl group, an octavinyl group, an octaoctyl group, an octadodecyl group, an octaepoxycyclohexylethyl group and an acryloxypropyl group; The ladder silsesquioxane includes at least one of phenyl ladder polysilsesquioxane, methacryloxypropyl ladder polysilsesquioxane, glycidyl ether epoxy ladder polysilsesquioxane, and 2-(3,4-epoxyhexyl)ethyl ladder polysilsesquioxane.

[0043] The heat stabilizer in the formulation of the present invention is a conventional heat stabilizer in the prior art, preferably at least one of iron oxide and cerium oxide.

[0044] The catalyst in the formulation of the present invention is a conventional catalyst in the prior art, preferably at least one of chloroplatinic acid, platinum-methylvinylsiloxane coordination complex and platinum-alkynyl complex.

[0045] The solvent in the formulation of the present invention is a conventional solvent in the prior art, preferably at least one of xylene, toluene and cyclohexane.

[0046] In the following examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0047] The highly flame-retardant silicone impregnating materials for high-sensitive resistors provided in Examples 1 to 6 of the present invention have components and mass fractions as shown in Table 1: The preparation method is as follows: The vinyl silicone oil, catalyst, inhibitor, tackifier, reinforcing resin, flame retardant, ceramic additive and solvent are weighed in parts by mass respectively, added into a high-speed disperser and dispersed for 60 minutes to 90 minutes to obtain a first mixture; a cross-linking agent is added into the high-speed disperser containing the first mixture, and stirred for 10 minutes to 15 minutes to obtain a second mixture; the obtained second mixture is subjected to a vacuum degassing treatment for 30 minutes to obtain a high flame retardant silicone impregnating material for a varistor, and the viscosity of the obtained high flame retardant silicone impregnating material for a varistor is 50000 mpa·s to 100000 mpa·s (6 r / min), 15000 mpa·s to 30000 mpa·s (60 r / min).

[0048] During dipping, the varistor is immersed in the above-mentioned highly flame-retardant silicone impregnation material. When pulling, the varistor ceramic piece needs to be slightly shaken to obtain a varistor of specified thickness (coating thickness 0.3mm~0.5mm). The reason is that the shaking process reduces the viscosity of the adhesive around the ceramic piece and increases its fluidity. The dipping is formed in one step, and the entire pulling process takes 3s~5s.

[0049] After drying the solvent at 60℃~80℃ for 30min, high temperature curing is performed at 100℃~160℃ for 1h~3h to obtain a dip-coated varistor.

[0050] The highly flame-retardant silicone impregnating material for varistor provided by the present invention can be applied to the encapsulation of varistors, the dip coating encapsulation of thermistors and the dip coating encapsulation of electronic components.

[0051] The rubber materials and dip-coated varistors in Examples 1 to 6 were tested, and the test items included overvoltage (without fuse) combustion test, coating withstand voltage test, and temperature cycle test.

[0052] Overvoltage (no fuse) flame retardant test: Apply 0.85 times the rated voltage to both ends of the dip-coated varistor. After the dip-coated varistor breaks down, continue to power on for 1 minute. Observe whether there is an open flame during the whole process, and record the time when the open flame starts to be generated.

[0053] The coating pressure resistance is measured using the method described in GB / T6663.1-2007; Temperature cycle test: -40℃×30min~125℃×30min, 1000 times.

[0054] The test results of Examples 1 to 6 are shown in Table 2: Table 2 Test results of dip-coated varistors

[0055] The present invention also provides comparative examples 1 to 4 to illustrate the superiority of the components and mass fractions in the present invention.

[0056] Comparative Example 1: The second flame retardant in Example 1 was completely replaced by the first flame retardant, and the other components remained unchanged.

[0057] Comparative Example 2: The first flame retardant in Example 1 was reduced to 10 parts, and the other components remained unchanged.

[0058] Comparative Example 3: The glass powder in Example 3 is replaced with glass powder of 300° C. to 600° C., and the other components remain unchanged.

[0059] Comparative Example 4: The organosilicon flame retardant in Example 1 was completely replaced by the first flame retardant, and the other components remained unchanged.

[0060] The rubber materials and dip-coated varistors in Comparative Examples 1 to 4 were tested, and the test items were overvoltage (without fuse) combustion test, coating withstand voltage, and temperature cycle test.

[0061] Overvoltage (no fuse) flame retardant test: Apply 0.85 times the rated voltage to both ends of the dip-coated varistor. After the varistor breaks down, continue to power on for 1 minute. Observe whether there is open flame during the whole process and record the time when the open flame starts.

[0062] The pressure resistance of the coating is determined using the method described in GB / T6663.1-2007.

[0063] Temperature cycle test: -40℃×30min~125℃×30min, 1000 times.

[0064] The test results of Comparative Examples 1 to 4 are shown in Table 3: Table 3 Test results of dip-coated varistors

[0065] From Table 1, Table 2 and Table 3, it can be seen that when there is no second flame retardant, the flame retardant effect of the high flame retardant silicone product is poor, and it burns under overpressure (no fuse); after reducing the total addition amount of different types of flame retardants, the flame retardant performance of the high flame retardant silicone product becomes worse, and it burns under overpressure (no fuse); after replacing the glass powder with glass powder of 300℃~600℃, the high flame retardant silicone product burns under overpressure (no fuse); when no silicone flame retardant is added, the flame retardant effect of the high flame retardant silicone product is poor, and it burns under overpressure (no fuse).

[0066] Compared with thermosetting silicone resin encapsulants with good flame retardancy, the high flame retardant silicone impregnating material for varistor provided by the present invention is a silicone material with better flexibility. For electronic products of larger sizes, it has better temperature cycling performance and does not crack after 1000 cycles. In addition, the high flame retardant silicone impregnating material for varistor provided by the present invention is an addition-type silicone product, which does not release small molecules during curing, forms a dense film after curing, and has a higher pressure resistance of the coating. However, small molecules are released when silicone resin is cured, and there are many small pores inside the coating film, resulting in a low pressure resistance of the coating.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A highly flame-retardant silicone impregnating material for a varistor, characterized in that: Its composition and mass fraction are as follows: Vinyl silicone oil, 15 to 40 parts; Reinforcing resin, 0-10 parts; Inorganic flame retardant, 20 to 40 parts; Ceramizing agent, 30 to 60 parts; Silicone flame retardant, 1 to 10 parts; Thickener, 0.5 to 4 parts; Catalyst, 0.1 to 0.3 parts; Cross-linking agent, 1 to 5 parts; Inhibitor, 0.1 to 0.5 parts; Heat stabilizer, 1 to 5 parts; Solvent: 10 to 20 parts.

2. The highly flame-retardant silicone impregnating material for varistor according to claim 1, characterized in that: The vinyl silicone oil is a single viscosity vinyl silicone oil or is compounded from vinyl silicone oils of different viscosities; Wherein, when the vinyl silicone oil is compounded with vinyl silicone oils of different viscosities, the viscosity of the vinyl silicone oil is ≥1000 mPa·s.

3. The highly flame-retardant silicone impregnating material for varistor according to claim 2, characterized in that: The vinyl silicone oil is vinyl polysiloxane, and the vinyl polysiloxane includes at least one of vinyl-terminated polydimethylsiloxane, vinyl-terminated polymethylphenylsiloxane and vinyl-terminated boron-containing silicone oil.

4. The highly flame-retardant silicone impregnating material for varistor according to claim 1, characterized in that: The reinforcing resin is MQ silicone resin, and the MQ silicone resin is any one of methyl vinyl MQ silicone resin and methyl phenyl vinyl MQ silicone resin.

5. The highly flame-retardant silicone impregnating material for varistor according to claim 1, characterized in that: The inorganic flame retardant is compounded by a first flame retardant and a second flame retardant, wherein the first flame retardant is at least one of aluminum hydroxide and magnesium hydroxide, and the second flame retardant is at least one of basic magnesium carbonate, basic zinc carbonate and zinc hydroxystannate; Wherein, the mass ratio of the second flame retardant to the inorganic flame retardant is 1 / 5 to 1 / 3.

6. The highly flame-retardant silicone impregnating material for varistor according to claim 5, characterized in that: The inorganic flame retardant is used after being treated with the first coupling agent, and the treatment process is as follows: Adding an inorganic flame retardant to a mixing device, spraying the first coupling agent / ethanol solution into the mixing device when mixing the inorganic flame retardant, and baking at 100° C. to 180° C. for 1 h to 3 h after mixing; Wherein, the mass ratio of the first coupling agent to ethanol is 1:20 to 1:10; The first coupling agent is at least one of KH560, KH570, A171 and A172.

7. The highly flame-retardant silicone impregnating material for varistor according to claim 1, characterized in that: The ceramicizing additive includes at least three of mica powder, wollastonite, silica powder and glass powder; The glass powder has a melting point of 800°C to 1300°C, a particle size of 325 mesh to 500 mesh, and an aspect ratio of 10:1 to 20:1; The particle size of the mica powder is 325 mesh to 800 mesh; The wollastonite has a particle size of 325 mesh to 1250 mesh and an aspect ratio of 10:1 to 20:1; The particle size of the silicon micropowder is 400-1000 meshes.

8. The highly flame-retardant silicone impregnating material for varistor according to claim 7, characterized in that: The ceramicizing agent is used after being treated with the second coupling agent, and the treatment process is as follows: Adding a ceramicizing agent to a mixing device, spraying a second coupling agent / ethanol solution when the ceramicizing agent is mixed in the mixing device, and baking at 100° C. to 180° C. for 1 to 3 hours after mixing; Wherein, the mass ratio of the second coupling agent to ethanol is 1:20 to 1:10; The second coupling agent is at least one of KH560, KH570, A171 and A172.

9. The highly flame-retardant silicone impregnating material for varistor according to claim 1, characterized in that: The organosilicon flame retardant includes cage-type silsesquioxane and ladder-type polysilsesquioxane; Wherein, the cage-type silsesquioxane includes at least one of a glycidyloxy group, a methacryloxy group, an octaphenyl group, an octaisobutyl group, an octavinyl group, an octaoctyl group, an octadodecyl group, an octaepoxycyclohexylethyl group and an acryloxypropyl group; The ladder silsesquioxane includes at least one of phenyl ladder polysilsesquioxane, methacryloxypropyl ladder polysilsesquioxane, glycidyl ether epoxy ladder polysilsesquioxane, and 2-(3,4-epoxyhexyl)ethyl ladder polysilsesquioxane.

10. A method for preparing a highly flame-retardant silicone impregnating material for a varistor, characterized in that: The method for preparing the highly flame-retardant silicone impregnating material for a varistor according to any one of claims 1 to 9 comprises the following steps: S100, weighing vinyl silicone oil, catalyst, inhibitor, tackifier, reinforcing resin, flame retardant, ceramic additive and solvent according to the mass parts of the formula, adding them into a disperser, and dispersing for 60 minutes to 90 minutes to obtain a first mixture; S200, adding a crosslinking agent into the disperser containing the first mixture, stirring for 10 min to 15 min to obtain a second mixture; S300, performing vacuum degassing treatment on the obtained second mixture to obtain a highly flame-retardant silicone impregnating material for a varistor.