Long-acting photocatalyst coating as well as preparation method and application thereof

By using a combination technology of inorganic coating and nanotitanium oxide coating in the photocatalyst coating, the early failure problem caused by embedding and light damage is solved, and the uniform spread and firm combination of nanotitanium oxide particles is achieved. The service life of photocatalysts is extended and its efficiency is improved.

CN118909465AActive Publication Date: 2024-11-08BEIJING YINHEHUI NEW MATERIAL TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411010348.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing photocatalyst coatings have poor sterilization and disinfection due to the embedding of resin or emulsion, and the adhesive is destroyed under light conditions and cannot be effective for a long time.

Method used

Using a combination of inorganic coating and nanotitanium oxide coating, an inorganic coating with a silicon oxide network structure is provided on the substrate surface, and a nanotitanium oxide coating is provided on it, using alcohol solvents in the inorganic coating and nanotitanium oxide. The liquid phase fusion of the dispersion liquid allows the nano-titanium oxide particles to spread evenly and physically embedded in the inorganic coating, forming chemical bond connections to avoid embedding and light damage.

Benefits of technology

The uniform spread and firm combination of nano-titanium oxide particles is achieved, the service life of photocatalysts is extended, the efficiency of sterilization, disinfection and decomposition of organic pollutants is improved, and the early failure of the binder is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964154090000161
    Figure BDA0004964154090000161
  • Figure HDA0004964154100000011
    Figure HDA0004964154100000011
Patent Text Reader

Abstract

The invention provides a long-acting photocatalyst coating and a manufacturing method and application thereof. The long-acting photocatalyst coating comprises: a substrate; the inorganic coating is arranged on the surface of the substrate; the inorganic coating comprises a silicon oxide network structure; the nano titanium oxide coating is arranged on the surface of the inorganic coating; the preparation method comprises the following steps: arranging the inorganic coating on the surface of the substrate; when the inorganic coating is in a wet state, a nano titanium oxide coating is arranged on the surface of the inorganic coating; the nano titanium oxide coating is water or alcohol dispersion liquid of nano titanium oxide; the nano titanium oxide coating and the inorganic coating are fused and dried, and the long-acting photocatalyst coating is obtained. The technical problem to be solved by the invention is how to uniformly disperse nano titanium oxide particles on the surface of an object, so that the nano titanium oxide particles not only have a photocatalyst function, but also are durable and do not fall off, thereby being more practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional coating manufacturing, and in particular relates to a long-acting photocatalyst coating and a manufacturing method and application thereof. Background Art

[0002] Photocatalyst is a general term for optical semiconductor materials with photocatalytic functions, represented by nano-scale titanium dioxide. It is coated on the surface of the substrate and produces a strong catalytic degradation function under the action of ultraviolet light. It can effectively degrade toxic and harmful gases in the air, effectively kill a variety of bacteria, and decompose and harmlessly treat toxins released by bacteria or fungi; it also has the functions of removing formaldehyde, deodorizing, anti-fouling, and purifying the air.

[0003] Most of the photocatalysts on the market today disperse nano titanium dioxide photocatalyst particles together with other additives in resin or emulsion. The resin or emulsion is a medium for dispersing the photocatalyst particles and a binder for firmly bonding the photocatalyst particles to the surface of an object. However, due to the embedding of the resin or emulsion, the sterilization and disinfection effect of the photocatalyst is poor. At the same time, the photocatalyst will act on organic matter such as the resin or emulsion under light conditions, causing the binder to be destroyed, thereby rendering the coating ineffective and unable to have a long-lasting photocatalytic effect. Summary of the invention

[0004] The main purpose of the present invention is to provide a long-lasting photocatalyst coating and its manufacturing method and application. The technical problem to be solved is how to evenly disperse nano-titanium oxide particles on the surface of an object so that it not only has photocatalytic function but is also durable and will not fall off, thus being more suitable for practical use.

[0005] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. A long-lasting photocatalyst coating proposed in the present invention comprises:

[0006] substrate;

[0007] An inorganic coating is disposed on the surface of the substrate; the inorganic coating comprises a silicon oxide network structure;

[0008] The nano titanium oxide coating is arranged on the surface of the inorganic coating.

[0009] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.

[0010] Preferably, in the aforementioned long-acting photocatalyst coating, the thickness of the nano titanium oxide coating is ≤100 nm; and the particle size of the nano titanium oxide particles in the nano titanium oxide coating is 5 to 100 nm.

[0011] Preferably, in the aforementioned long-lasting photocatalyst coating, the thickness of the nano-titanium oxide coating is ≤50 nm; and the particle size of the nano-titanium oxide particles in the nano-titanium oxide coating is 5 to 50 nm.

[0012] Preferably, the raw materials of the coating for forming the inorganic coating of the aforementioned long-lasting photocatalyst coating include: 39-59wt% of organic alkoxysilane, 39-59wt% of silica sol, and 0.5-2wt% of functional additive; the total amount of the organic alkoxysilane, silica sol and functional additive is 100%; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, and m is a natural number from 0 to 3.

[0013] Preferably, the raw materials of the coating for forming the inorganic coating of the aforementioned long-lasting photocatalyst coating include: 70-80wt% of solution; 5-10wt% of functional additives, the functional additives are selected from potassium titanate, aluminum oxide or a combination of the two; 10-20wt% of inorganic pigments; 0.5-2.0wt% of other functional additives; the raw materials of the solution include the following ingredients: 30-40wt% of organic alkoxy silane, 15-20wt% of organic solvent, 25-30wt% of silica sol; the organic alkoxy silane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, m is a natural number from 0 to 3; the above percentages are the mass percentages of each raw material in the total weight of the inorganic coating.

[0014] Preferably, the raw materials of the coating for forming the inorganic coating of the aforementioned long-lasting photocatalyst coating include: 30-99.9% inorganic resin; 0.1-70% silicon nitride; 0-10% functional additives; 0-18% inorganic pigments; 0-2% other functional additives; the total amount of the coating is 100%; wherein the inorganic resin is obtained by mixing and reacting an organic alkoxysilane, an organic solvent and a silica sol, extracting alcohol, and adding deionized water; the mass ratio of the organic alkoxysilane, the organic solvent and the silica sol is 1-1.6:0.5-0.8:1; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, and m is a natural number of 0 to 3; the inorganic resin is an acidic cationic system; the VOC content of the inorganic resin is ≤10% by mass percentage; and the functional additive is selected from at least one of potassium titanate, aluminum oxide and nano-silicon oxide.

[0015] Preferably, in the aforementioned long-lasting photocatalyst coating, the coating material forming the nano titanium oxide coating is a water and / or alcohol dispersion of nano titanium oxide.

[0016] The purpose of the present invention and the technical problem solved by the present invention are also achieved by adopting the following technical solutions. According to a method for preparing a long-lasting photocatalyst coating proposed by the present invention, the method comprises the following steps:

[0017] S11: placing an inorganic coating on the surface of the substrate;

[0018] S12: when the inorganic coating is in a wet state, a nano titanium oxide coating is provided on the surface of the inorganic coating; the nano titanium oxide coating is a water and / or alcohol dispersion of nano titanium oxide;

[0019] S13 nano titanium oxide coating is fused with inorganic coating and dried to obtain a long-lasting photocatalyst coating.

[0020] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.

[0021] Preferably, in the aforementioned preparation method, the inorganic coating being in a wet state refers to a state in which the inorganic coating has not yet dried on the surface.

[0022] The purpose of the present invention and the technical problems solved therein are also achieved by adopting the following technical solutions: The present invention proposes an application of a long-lasting photocatalyst coating in the field of sterilization or self-cleaning.

[0023] By means of the above technical solution, the long-lasting photocatalyst coating and its manufacturing method and application proposed by the present invention have at least the following advantages:

[0024] The long-acting photocatalyst coating provided by the present invention and its manufacturing method and application are achieved by arranging an inorganic coating on a base material and then arranging a nano-titanium oxide coating on the inorganic coating. By limiting the preparation process that the nano-titanium oxide coating is arranged when the inorganic coating is still in a wet state, the nano-titanium oxide particles in the nano-titanium oxide coating can be evenly spread on the surface of the inorganic coating, thus overcoming the defect in the prior art that the nano-titanium oxide particles are difficult to evenly spread on the surface of an object. Regarding the applicant's discovery, the applicant speculates that the reason may be: since the inorganic coating that forms the inorganic coating includes organic alkoxysilane and silica sol, the two can form water and / or alcohol solvents during the self-condensation reaction; the nano-titanium oxide coating that forms the nano-titanium oxide coating is a water and / or alcohol dispersion of nano-titanium oxide, and the nano-titanium oxide coating is set when the inorganic coating is still in a wet state, therefore, the water and / or alcohol solvent added to the inorganic coating or generated by the self-condensation reaction and the dispersion medium water and / or alcohol solvent in the nano-titanium oxide dispersion can be infiltrated into each other by the water-alcohol solvent, and the nano-titanium oxide particles in the dispersion can be evenly spread on the surface of the inorganic coating by the liquid phase fusion method. The above technical scheme of the present invention can make the nano titanium oxide particles evenly spread on the surface of the inorganic coating, and the two are dried after being completely fused; on the one hand, the nano titanium oxide particles can be physically embedded in the inorganic coating; on the other hand, the titanium element in the nano titanium oxide particles can exist in a tetravalent form, which is chemically bonded with the silicon oxygen bond in the silicon oxide network structure in the inorganic coating through chemical bonding, so that the nano titanium oxide particles are firmly bound to the surface of the inorganic coating; after the two are fused, they are dried together, and at this time, the nano titanium oxide particles are firmly bound to the surface of the object to form a long-lasting photocatalyst coating. At the same time, since the preparation process is to prepare the inorganic coating first, and then set the nano titanium oxide particles on the surface of the inorganic coating, the nano titanium oxide particles are in the upper position, which can better avoid the nano titanium oxide particles from being embedded, thereby greatly avoiding or reducing the technical effect of the nano titanium oxide particles as a photocatalyst and the loss of efficiency in sterilization, disinfection, and decomposition of organic pollutants. Furthermore, since the connecting medium between the substrate surface and the nano-titanium oxide particles is an inorganic coating, it is completely possible to avoid the nano-titanium oxide particles from acting on the connecting medium and being damaged when decomposing organic matter under the action of light, making the inorganic coating difficult to be damaged, greatly prolonging its bonding and fixing time for the nano-titanium oxide particles, thereby greatly prolonging the service life of the nano-titanium oxide particles as a photocatalyst, and can play its role in sterilization, disinfection and decomposition of organic pollutants for a long time.

[0025] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is the energy spectrum component analysis spectrum of the inorganic coating varnish of Preparation Example 1-3 of the present invention. DETAILED DESCRIPTION

[0027] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the following is a detailed description of a long-lasting photocatalyst coating and its manufacturing method and its specific implementation method, structure, characteristics and effects proposed by the present invention in combination with the preferred embodiments.

[0028] The present invention provides a long-lasting photocatalyst coating, which comprises a substrate, an inorganic coating and a nano titanium oxide coating in sequence.

[0029] The substrate is mainly used as a carrier of the long-lasting photocatalyst coating; the carrier can be various organic and inorganic materials such as glass, plastic, paint or metal. As long as it can carry the coating, it can be used as a substrate, and the present invention does not make specific restrictions on it. Since photocatalysts can decompose organic matter under light conditions, they have only been applied to the surfaces of non-organic materials such as glass and metal for many years. The present invention uses the technical means of first setting an inorganic coating on the surface of the substrate, and blocks the reaction of the nano-titanium oxide coating to the substrate through physical isolation, so that the long-lasting photocatalyst coating of the present invention can be widely used on various organic and inorganic materials, greatly expanding the application scenarios of photocatalysts; that is, the technical solution of the present invention can not only set the long-lasting photocatalyst coating on the surface of glass, metal, and stainless steel materials, but can even set it on organic coatings, such as existing car paint, train paint, etc. Surface to achieve a self-cleaning effect.

[0030] The inorganic coating is arranged on the surface of the substrate; the nano titanium oxide coating is arranged on the surface of the inorganic coating. The inorganic coating includes a silicon oxide network structure. It should be particularly noted that the silicon oxide included in the inorganic coating of the present invention is not silicon oxide particles, but a silicon-oxygen-silicon network structure formed by the self-condensation of silanol; in order to illustrate the morphological structure of silicon oxide in the inorganic coating in the technical solution of the present invention, in a specific embodiment of the present invention, the inorganic coating is made into a varnish, and the inorganic coating formed after its self-condensation into a film is subjected to energy spectrum component analysis, and the spectrum is shown in the attached figure. Figure 1 As shown, the results of energy spectrum component analysis are as follows as shown in Table 1:

[0031] Table 1

[0032] element Weight percentage, % Atomic percentage, % OK 33.26 46.66 S K 66.74 53.34

[0033] Note: The test area is the transparent coating surface

[0034] The spectrum is processed as follows:

[0035] Peak that may be overlooked: 2.150keV

[0036] Processing options: All analyzed elements (normalized)

[0037] Repeat 3 times

[0038] Standard samples: O SiO2, Si SiO2

[0039] In order to avoid the nano titanium oxide particles being embedded and affecting their effect as photocatalysts, the coating for forming the nano titanium oxide coating is preferably a water and / or alcohol dispersion of nano titanium oxide, in which no other raw materials such as pigments, fillers and resins are added; the nano titanium oxide particles in the present invention are in a dispersed state rather than a dissolved state in water and / or alcohol solvents, and the dispersion formed is transparent in appearance, but it is actually a suspension; or, the nano titanium oxide particles in the present invention are in a titanium sol state similar to a silica sol structure in water and / or alcohol solvents, and the dispersion formed is transparent in appearance, but it is actually a sol. Although the solid content of the nano titanium oxide dispersion will have a certain effect on the gloss of the coating, it will not affect its effect as a photocatalyst, so the present invention does not strictly limit the solid content of the dispersion, as long as it can stably store the dispersion and can easily and evenly spread on the surface of the inorganic coating.

[0040] The present invention limits the provision of the nano titanium oxide coating on the surface of the inorganic coating. On the one hand, the applicant surprisingly found that the dispersion of nano titanium oxide can be easily and evenly spread on the surface of the inorganic coating that is still in a wet state. Although its mechanism cannot be accurately determined, the applicant speculates that the possible reasons are: the solvent used in the inorganic coating that forms the inorganic coating is an alcohol solvent, or, even if the inorganic coating is not added with any solvent, it will generate an alcohol solvent during the silanol self-condensation reaction; the nano titanium oxide coating that forms the nano titanium oxide coating is a water and / or alcohol dispersion of nano titanium oxide. Due to the physical and / or chemical properties of alcohol solvents and water, the two can infiltrate each other under wet conditions, and in the liquid During the fusion process, the nano-titanium oxide particles in the dispersion are evenly spread on the surface of the inorganic coating, thus overcoming the technical difficulty that the nano-titanium oxide particles are difficult to evenly spread on the surface of an object; it may also be due to the positive and negative charge interaction, or the anion and cation interaction, between the inorganic coating and the dispersion of the nano-titanium oxide; on the other hand, due to the unique composition of the inorganic coating itself, which is different from the general organic binders such as resins and emulsions, it will not be decomposed and destroyed by the nano-titanium oxide particles under the action of light, so that it can maintain the inorganic coating for a long time. The bonding and fixing effect of the nano-titanium oxide particles can be exerted for a long time, that is, the long-lasting photocatalyst coating of the present invention is a semi-permanent coating.

[0041] In order to enable the long-lasting photocatalyst coating of the present invention to be applied to the surface of transparent materials such as glass, and to avoid or reduce the influence on the transparency of the substrate, the present invention preferably adopts the inorganic coating as a transparent coating, and the nano titanium oxide coating as a transparent coating. The raw materials of the coating forming the inorganic coating preferably include: 39-59wt% of organic alkoxysilane, 39-59wt% of silica sol, and 0.5-2wt% of functional additive; the total amount of the organic alkoxysilane, silica sol and functional additive is 100%; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, and m is a natural number of 0 to 3; the functional additives include but are not limited to wetting agents, leveling agents, and the like.

[0042] In order to ensure that the dispersion of nano titanium oxide can be well spread on the surface of the inorganic coating, the inorganic coating can also be a color paint; the raw materials of the coating that preferably forms the inorganic coating of the present invention include: 70-80wt% of solution; 5-10wt% of functional additives, the functional additives are selected from potassium titanate, aluminum oxide or a combination of the two; 10-20wt% of inorganic pigments; 0.5-2.0wt% of other functional additives; the raw materials of the solution include the following ingredients: 30-40wt% of organic alkoxy silane, 15-20wt% of organic solvent, 25-30wt% of silica sol; the organic alkoxy silane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2The total number is 4, m is a natural number of 0 to 3; the above percentages are the mass percentages of each raw material in the total weight of the inorganic coating; for details, please refer to the applicant's prior related patent: Announcement No. CN105038335B, patent name "A room temperature curing inorganic coating and its manufacturing method". Alternatively, the raw materials of the coating that preferably forms the inorganic coating of the present invention include: 30 to 99.9% inorganic resin; 0.1 to 70% silicon nitride; 0 to 10% functional additives; 0 to 18% inorganic pigments; 0 to 2% other functional additives; the total amount of the coating is 100%; wherein the inorganic resin is obtained by mixing and reacting an organic alkoxysilane, an organic solvent and a silica sol, extracting alcohol, and adding deionized water; the mass ratio of the organic alkoxysilane, the organic solvent and the silica sol is 1 to 1.6: 0.5 to 0.8: 1; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, and m is a natural number of 0 to 3; the inorganic resin is an acidic cationic system; the VOC content of the inorganic resin is ≤10% by mass percentage; the functional additive is selected from at least one of potassium titanate, aluminum oxide and nano-silicon oxide; for details, please refer to the applicant's prior related patent: announcement number CN112280344B, patent name "Ceramic composite coating, anti-virus ceramic composite coating and preparation method and coating thereof".

[0043] When the nano-titanium oxide dispersion is still in a wet state, the alcohol solvent contained in the inorganic coating or the alcohol solvent generated by the self-condensation of the inorganic coating can mutually infiltrate the water and / or alcohol solvent in the nano-titanium oxide dispersion, and the nano-titanium oxide particles in the dispersion are evenly spread on the surface of the inorganic coating under the action of liquid fusion, thereby achieving uniform spreading of the nano-titanium oxide particles on the surface of the object. As the paint dries and the coating is formed, the nano-titanium oxide particles are firmly bonded to the surface of the object by the inorganic coating. Moreover, after the nano-titanium oxide paint dries, it only contains the nano-titanium oxide particles, which are located on the outermost surface of the coating. Therefore, the nano-titanium oxide particles will not be buried by any substance, so that the nano-titanium oxide particles can play the role of photocatalyst to the maximum extent. Furthermore, since the nano-titanium oxide particles can decompose organic matter under light conditions when used as photocatalysts, and the material bonding the nano-titanium oxide particles is an inorganic coating, which does not contain organic matter in the traditional sense such as emulsions and resins, the nano-titanium oxide particles will not act on the inorganic coating when they act as photocatalysts, that is, the inorganic coating bonding the nano-titanium oxide particles will not be damaged, so the adhesion time of the nano-titanium oxide particles on the surface of the object can be greatly extended, so that it can play the photocatalytic effect for a long time.

[0044] In order to better realize the long-lasting photocatalytic effect of nano-titanium oxide particles, the present invention preferably has a particle size of 5 to 100 nm; if the particle size of the nano-titanium oxide particles is less than 5 nm, they may be embedded in the inorganic coating due to their small particle size, affecting their effectiveness as a photocatalyst; and if the particle size of the nano-titanium oxide particles is greater than 100 nm, they may be difficult to embed in the silicon-oxygen-silicon network structure of the inorganic coating due to their large particle size, thereby affecting their bonding strength with the inorganic coating, causing the nano-titanium oxide particles to easily fall off, affecting their service life as a photocatalyst.

[0045] The applicant has found through a large number of experiments that the particle size of the nano titanium oxide particles is more preferably 5-50nm, 50-100nm; the particle size of the nano titanium oxide particles is more preferably 5-20nm, 20-40nm, 40-60nm, 60-80nm, 80-100nm; the particle size of the nano titanium oxide particles is more preferably 5-10nm, 10-15nm, 15-20nm, 20-25nm, 25-30nm, 30-35nm, 35-40nm, 40-45nm, 45-50nm, 50-55nm, 55-60nm, 60-65nm, 65-70nm, 70-75nm, 75-80nm, 80-85nm, 85-90nm, 90-95nm, 95-100nm.

[0046] In order to better achieve the photocatalytic efficiency of nano titanium oxide particles, the present invention preferably has a thickness of ≤100nm for the nano titanium oxide coating. If the thickness of the nano titanium oxide coating is too thick, the nano titanium oxide particles may be embedded in each other, affecting its effectiveness as a photocatalyst. Therefore, the thickness is as thin as possible to match the particle size of the nano titanium oxide particles to improve its efficiency. The applicant has found through a large number of experiments that the thickness of the nano titanium oxide coating is more preferably ≤80nm, ≤60nm, ≤40nm, ≤20nm.

[0047] The present invention also provides a method for preparing a long-lasting photocatalyst coating, which comprises the following steps:

[0048] S11 sets an inorganic coating on the surface of the substrate; the inorganic coating can be the varnish as described above, or it can be the color paint as described above; when the inorganic coating is a varnish, no solvent is added thereto; when the inorganic coating is a color paint, the solvent added thereto is an alcohol solvent; the specific implementation form of the inorganic coating and the color paint can refer to the applicant's prior application: the patent with announcement number CN105038335B, the patent name is "A room temperature curing inorganic coating and its manufacturing method" and the patent with announcement number CN112280344B, the patent name is "Ceramic composite coating, anti-virus ceramic composite coating and its preparation method and coating". Any formula of the inorganic coating, as long as its solvent can interact with water to make the nano-oxidized particles evenly spread, and at the same time includes a silicon-oxygen-silicon network structure, on the one hand, the nano-oxidized particles can be physically embedded and combined, and on the other hand, the titanium in the nano-oxidized particles can be chemically bonded to the silicon-oxygen-silicon network structure, thereby improving the bonding strength of the inorganic coating to the nano-oxidized particles.

[0049] S12: When the inorganic coating is in a wet state, a nano titanium oxide coating is arranged on the surface of the inorganic coating; the nano titanium oxide coating is a water and / or alcohol dispersion of nano titanium oxide; the present invention limits the solvent of the nano titanium oxide coating to water and / or alcohol, and particularly limits the timing of setting the nano titanium oxide coating to when the inorganic coating is in a wet state. On the one hand, this is to enable the nano-oxidized particles uniformly dispersed in the nano titanium oxide dispersion to be uniformly spread on the surface of the object under the action of the water-alcohol solvent through the coordinated action of the water and / or alcohol in the nano titanium oxide coating and the alcohol solvent in the inorganic coating. On the other hand, the nano titanium oxide coating is limited to a dispersion of nano titanium oxide so that it does not contain other raw materials, so as to avoid or reduce the embedding of the nano-oxidized particles by other raw materials and affect its effectiveness as a photocatalyst.

[0050] S13: Through the definition of the above two steps, the nano titanium oxide coating and the inorganic coating are deeply integrated in the form of physical embedding and chemical bonding, and after drying, a long-lasting photocatalyst coating can be obtained.

[0051] In order to make the inorganic coating and the nano titanium oxide coating interact better and facilitate the uniform spreading of the nano oxidized particles, the present invention preferably states that the inorganic coating is in a wet state, which means that the inorganic coating has not yet dried on the surface. In specific operations, the nano titanium oxide coating can generally be set within 10 minutes after the inorganic coating is set, so that the nano titanium oxide coating is set on the surface of the inorganic coating before it dries on the surface, which can more fully allow the alcohol solvent and water to infiltrate each other, and the nano oxidized particles can be evenly spread on the surface of the inorganic coating through liquid phase fusion.

[0052] The present invention also proposes an application of the aforementioned long-acting photocatalyst coating in the field of sterilization or self-cleaning.

[0053] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.

[0054] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods well known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the common meanings understood by ordinary technicians in the field to which the present invention belongs.

[0055] Preparation Example 1-1

[0056] This preparation example provides an inorganic coating varnish, and the preparation method is as follows:

[0057] 1) Preparation of inorganic solution: 59 parts of methyltrimethoxysilane and 39 parts of silica sol are mixed together, stirred at 40-50°C for 5-10 minutes, and the mixed solution of alkoxysilane and silica sol undergoes a chemical reaction, generating heat. As the reaction proceeds, the turbid state gradually changes into a transparent liquid, and an inorganic solution in a sol state is obtained;

[0058] 2) Stirring the mixed solution: adding 2 parts of an organosilicon wetting agent and a leveling agent to the inorganic solution, mixing and stirring together to form an inorganic coating mixture;

[0059] 3) Extracting the coating: Filter the above-mentioned uniformly stirred substances through a filter net of a certain size, extract the particles, and finally complete the coating.

[0060] Preparation Example 1-2

[0061] This preparation example provides an inorganic coating varnish, and its preparation method is the same as that of Preparation Example 1-1. Its raw materials include the following components: 39 parts of tetraethoxysilane, 59 parts of silica sol, and 2 parts of an organosilicon wetting agent and a leveling agent.

[0062] Preparation Example 1-3

[0063] This preparation example provides an inorganic coating varnish, and its preparation method is the same as that of Preparation Example 1-1, and its raw materials include the following components: 20 parts of methyltrimethoxysilane, 30 parts of tetraethoxysilane, 49.5 parts of silica sol, and 0.5 parts of organic silicon wetting agent and leveling agent; the inorganic coating varnish of the preparation example is subjected to energy spectrum component analysis, and the results are as shown in the attached Figure 1 shown.

[0064] Preparation Example 2-1

[0065] This preparation example provides an inorganic coating color paint, and the preparation method is as follows:

[0066] 1) Preparation of inorganic solution: 28 parts of an organic silane selected from one or a mixture of methyltrimethoxysilane or tetraethoxysilane, in this preparation example, methyltrimethoxysilane, 14 parts of ethanol, and 28 parts of silica sol are mixed together, and stirred at a temperature of 40 to 50° C. for 5 to 10 minutes. The mixed solution of alkoxysilane and silica sol undergoes a chemical reaction, generating heat. As the reaction proceeds, the turbid state gradually changes into a transparent liquid, thereby obtaining an inorganic solution in a sol state;

[0067] 2) Preparation of inorganic resin: The inorganic solution is evacuated at 40-50° C. for 5 min, and deionized water is added to make up for the amount of solvent separated by alcohol extraction to obtain an inorganic resin; the VOC content of the inorganic resin is 8.7% and the solid content is 28%;

[0068] 3) Stirring the mixed solution: Mix the inorganic resin and other raw materials together to form an inorganic ceramic mixture; in terms of mass percentage, the inorganic ceramic mixture includes: 70% inorganic resin, 8% silicon nitride, 2% mixture of one or two selected from potassium titanate, aluminum oxide or nano silicon oxide, in this preparation example, 1% potassium titanate and 1% aluminum oxide are selected; 18% titanium dioxide, 2% rare earth mineral powder; the silicon nitride particle size is 1 μm to 3 μm; the particle size of the other added powders is less than 800 nm;

[0069] 4) Homogenization: the inorganic ceramic mixture is placed in a homogenizer and stirred at high speed for 0.1 to 2 hours to homogenize the particles;

[0070] 5) Extracting the coating: Filter the above-mentioned uniformly stirred substances through a filter net of a certain size, extract the particles, and finally complete the coating.

[0071] Preparation Example 2-2

[0072] This preparation example provides an inorganic coating, the preparation method of which is the same as that of Preparation Example 2-1, and the raw materials thereof include the following components:

[0073] 85% inorganic resin; the raw materials of the inorganic resin include the following components: 40.8 parts of tetraethoxysilane, 18.7 parts of ethanol, and 25.5 parts of silica sol; the silica particle size in the silica sol is 10 to 50 nm; the VOC content of the inorganic resin is 9.6%, and the solid content is 25%;

[0074] 5% silicon nitride; the silicon nitride particle size is 1 μm to 3 μm;

[0075] Potassium titanate 5%, nano silicon oxide 1%, aluminum oxide 4%; the particle size of other added powders is less than 800nm.

[0076] Preparation Example 2-3

[0077] This preparation example provides an inorganic coating, the preparation method of which is the same as that of Preparation Example 2-1, and the raw materials thereof include the following components:

[0078] 80% inorganic resin; the raw materials of the inorganic resin include the following components: 26.6 parts of tetraethoxysilane and 11.4 parts of methyltrimethoxysilane, 18 parts of ethanol, and 24 parts of silica sol; the silica particle size in the silica sol is 10 to 50 nm; the VOC content of the inorganic resin is 7.3%, and the solid content is 30%;

[0079] 13% silicon nitride; the silicon nitride particle size is 0.5 μm to 3 μm;

[0080] Alumina 3%, nano silicon oxide 1%, potassium titanate 2%, rare earth mineral powder 1%; the particle size of other added powders is less than 800nm.

[0081] Preparation Example 2-4

[0082] This preparation example provides an inorganic coating, the preparation method of which is the same as that of Preparation Example 2-1, and the raw materials thereof include the following components:

[0083] 99.9% inorganic resin; the raw materials of the inorganic resin include the following components: 43.9 parts of tetraethoxysilane, 21 parts of ethanol, and 35 parts of silica sol; the silica particle size in the silica sol is 10 to 50 nm; the VOC content of the inorganic resin is 7.0% and the solid content is 32%;

[0084] 0.1% silicon nitride; the silicon nitride particle size is 100-200nm.

[0085] Preparation Example 2-5

[0086] This preparation example provides an inorganic coating, the preparation method of which is the same as that of Preparation Example 2-1, and the raw materials thereof include the following components:

[0087] 50wt% inorganic resin; the raw materials of the inorganic resin include the following components: 12 parts of methyltriethoxysilane and 12 parts of tetraethoxysilane, 11 parts of ethanol, and 15 parts of silica sol; the silica particle size in the silica sol is 10 to 50nm; the VOC content of the inorganic resin is 8.4%, and the solid content is 29%;

[0088] 50% silicon nitride; the silicon nitride particle size is 2μm to 6μm.

[0089] Preparation Example 2-6

[0090] This preparation example provides an inorganic coating, the preparation method of which is the same as that of Preparation Example 2-1, and the raw materials thereof include the following components:

[0091] 30wt% inorganic resin; the raw materials of the inorganic resin include the following components: 13 parts of methyltriethoxysilane, 7 parts of ethanol, and 10 parts of silica sol; the silica particle size in the silica sol is 10 to 50nm; the VOC content of the inorganic resin is 9.3%, and the solid content is 26%;

[0092] 70% silicon nitride; the silicon nitride particle size is 2μm to 6μm.

[0093] Preparation Example 3-1

[0094] This preparation example provides an inorganic coating color paint, and the preparation method of the coating is as follows:

[0095] 1) In the stage of preparing the inorganic solution of this invention, 30wt% of organic silane, 15wt% of ethanol, and 30wt% of silica sol (referred to as silica gel) are mixed together from one or a mixture of methyltrimethoxysilane or tetraethoxysilane, and stirred at 40-50°C for about 5-10 minutes. The mixed solution of alkoxysilane and silica sol produces a chemical reaction, generating heat, and gradually changes from a turbid state to a transparent liquid as the reaction proceeds. At this time, in order to adjust the viscosity and reaction speed of the solution, one of methanol, ethanol, isopropanol or a mixture thereof is added, and after these processes, an inorganic solution in a sol state is prepared.

[0096] 2) In the mixed liquid stirring stage of this invention, one of the inorganic solution, potassium titanate or aluminum oxide prepared in the previous stage is selected as a functional additive 9wt%, titanium oxide pigment powder 15wt% and other functional additives 1wt% are mixed and stirred to form an inorganic coating mixed liquid.

[0097] 3) In the homogenization stage, the stirred material is placed into a homogenizer and stirred at high speed for 1-2 hours to homogenize the particles.

[0098] 4) The stage of extracting the coating, in which the homogenized material is filtered through a filter of a certain size, and the particles are extracted to finally complete the coating.

[0099] Preparation Example 3-2

[0100] This preparation example provides an inorganic coating, and its preparation method is the same as that of Preparation Example 3-1. The raw materials of the inorganic coating include the following components:

[0101] 70wt% inorganic solution; the raw materials of the inorganic solution include the following components: 30wt% tetraethoxysilane, 15wt% ethanol, 25wt% silica sol;

[0102] 10wt% of a functional aid, wherein the functional aid is a composition of potassium titanate and aluminum oxide, wherein the content of potassium titanate is 3%;

[0103] 19.5wt% inorganic pigment;

[0104] 0.5wt% of other functional additives; the other functional additive is tourmaline.

[0105] The above percentages are the weight percentages of each raw material to the total weight of the inorganic coating.

[0106] Preparation Example 3-3

[0107] This preparation example provides an inorganic coating, and its preparation method is the same as that of Preparation Example 3-1. The raw materials of the inorganic coating include the following components:

[0108] 80wt% inorganic solution; the raw materials of the inorganic solution include the following ingredients: 40wt% tetraethoxysilane and methyltrimethoxysilane composition, the weight ratio of tetraethoxysilane and methyltrimethoxysilane is 1:1, 15wt% ethanol, 25wt% silica sol;

[0109] 5wt% of a functional aid, wherein the functional aid is a composition of potassium titanate and aluminum oxide, wherein the content of potassium titanate is 4%;

[0110] 13 wt% inorganic pigment;

[0111] 2wt% of other functional additives; the other functional additive is tourmaline.

[0112] The above percentages are the weight percentages of each raw material to the total weight of the inorganic coating.

[0113] Preparation Example 3-4

[0114] This preparation example provides an inorganic coating, and its preparation method is the same as that of Preparation Example 3-1. The raw materials of the inorganic coating include the following components:

[0115] 80wt% inorganic solution; the raw materials of the inorganic solution include the following components: 30wt% methyltrimethoxysilane, 20wt% ethanol, 30wt% silica sol;

[0116] 6wt% of a functional aid, wherein the functional aid is a composition of potassium titanate and aluminum oxide, wherein the content of potassium titanate is 5%;

[0117] 13 wt% inorganic pigment;

[0118] 1wt% of other functional additives; the other functional additives are rare earth raw ore.

[0119] The above percentages are the weight percentages of each raw material to the total weight of the inorganic coating.

[0120] Preparation Example 3-5

[0121] This preparation example provides an inorganic coating, and its preparation method is the same as that of Preparation Example 3-1. The raw materials of the inorganic coating include the following components:

[0122] 74.5wt% of an inorganic solution; the raw materials of the inorganic solution include the following components: 30wt% of methyltriethoxysilane, 15wt% of ethanol, and 29.5wt% of silica sol;

[0123] 5wt% of a functional additive, wherein the functional additive is potassium titanate;

[0124] 20wt% inorganic pigment;

[0125] 0.5wt% of other functional additives; the other functional additives are rare earth raw ore.

[0126] The above percentages are the weight percentages of each raw material to the total weight of the inorganic coating.

[0127] Preparation Example 3-6

[0128] This preparation example provides an inorganic coating, and its preparation method is the same as that of Preparation Example 3-1. The raw materials of the inorganic coating include the following components:

[0129] 77wt% inorganic solution; the raw materials of the inorganic solution include the following components: 35wt% alkoxysilane, 15wt% ethanol, 27wt% silica sol;

[0130] 7wt% of a functional additive, wherein the functional additive is potassium titanate;

[0131] 15wt% inorganic pigment;

[0132] 1wt% of other functional additives; the other functional additives are a combination of tourmaline and rare earth ore, and the weight ratio of the two is 1:1.

[0133] The above percentages are the weight percentages of each raw material to the total weight of the inorganic coating.

[0134] The alkoxysilane has a molecular formula of R1mSi(OR2) 4-m It means that R2 is phenyl and m is 0.

[0135] Preparation Example 4-1

[0136] This preparation example provides a nano titanium oxide dispersion, wherein a dispersant is added to deionized water under stirring conditions, and then nano titanium oxide particles are added thereto and stirred evenly; the nano titanium oxide dispersion comprises the following ingredients: nano titanium oxide, 0.5%, with a particle size of 30 nm; deionized water, 98.5%; and a dispersant, 1%. The above percentages are the weight percentages of the raw materials in the total weight of the nano titanium oxide dispersion.

[0137] Preparation Example 4-2

[0138] This preparation example provides a nano titanium oxide dispersion, and its preparation method is the same as that of Preparation Example 4-1; the nano titanium oxide dispersion includes the following ingredients: nano titanium oxide, 1%, with a particle size of 20nm; deionized water, 99%; dispersant 1%; the above percentages are the weight percentages of each raw material to the total weight of the nano titanium oxide aqueous dispersion.

[0139] Preparation Example 4-3

[0140] This preparation example provides a nano titanium oxide dispersion, and its preparation method is the same as that of Preparation Example 4-1; the nano titanium oxide dispersion includes the following ingredients: nano titanium oxide, 5%, with a particle size of 10 nm; ethanol, 85%; dispersant 10%; the above percentages are the weight percentages of each raw material to the total weight of the nano titanium oxide aqueous dispersion.

[0141] Examples 1 to 15

[0142] The long-lasting photocatalyst coating was prepared according to the material configuration and process in the following table. An inorganic coating was firstly provided on the surface of the base material. Then, a nano titanium oxide coating was provided on the surface of the inorganic coating within 10 minutes and dried to obtain a long-lasting photocatalyst coating.

[0143] The long-lasting photocatalyst coating was tested for its performance in decomposing organic matter. The specific operation is as follows: prepare a saturated ethanol solution of methyl red (analytical grade), apply the solution on the test plate with a brush, and keep it away from light for 4 hours; then put the cured test plate into the test box for ultraviolet light test, the light source is UVA-340, and the irradiance is 0.68W / m 2, the temperature of the blackboard thermometer is 60±3℃; after 300h of ultraviolet light exposure, take out the test plate and compare it with a blank test plate not coated with methyl red saturated ethanol solution, and determine the color difference value according to 4.2.1 of GB / T1766.

[0144] The adhesion performance of the long-lasting photocatalyst coating after aging is tested. The specific operation is as follows: the test plate of the above-mentioned decomposition organic matter test and the blank test plate are used as test samples respectively. The test is carried out according to the cross-cutting test of GB / T 9286 paint and varnish coating. The sample is placed on a hard, flat table to avoid deformation of the sample. The knife is perpendicular to the surface of the sample, and the cutting tool is uniformly forced. A suitable spacing guide device is used to form 6 parallel cutting lines in the horizontal direction and 6 parallel cutting lines in the vertical direction on the coating at a uniform cutting rate. All cuts should be cut through to the surface of the substrate. Use a soft brush to gently sweep back several times and then forward several times along each diagonal line of the grid pattern. Place the center point of the 3M tape above the grid, parallel to a set of cutting lines, and then use your fingers to flatten the part of the tape above the grid area. The length of the tape should be at least 20mm longer than the grid. Within 5 minutes of applying the tape, hold the free end of the tape and tear it off steadily at an angle close to 60° within 0.5 to 1.0 seconds. Inspect the coated area under good lighting conditions.

[0145] In the above-mentioned Examples 1 to 15, the inorganic coating and the nano-titanium oxide dispersion are both sprayed; the specific process parameters and test results are shown in Table 2 below:

[0146] Table 2

[0147]

[0148] It can be seen from the above test data that after ultraviolet light irradiation, the color difference ΔE between the test plate coated with methyl red and the blank test plate not coated with methyl red is less than 3.0, that is, the long-acting photocatalyst coating of the present invention has good performance in decomposing organic matter and high efficiency in decomposing organic matter.

[0149] It can also be seen from the above test data that after 300 hours of ultraviolet irradiation, there is no change in the coating on the test panel painted with methyl red, and the adhesion of the nano-oxidized particles is still firm without any decrease in adhesion.

[0150] The technical features in the claims and / or the specification of the present invention may be combined, and the combination is not limited to the combination obtained by reference in the claims. The technical solution obtained by combining the technical features in the claims and / or the specification is also within the protection scope of the present invention.

[0151] The above description is only a preferred preparation example of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above preparation example according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A long-lasting photocatalyst coating, characterized in that: It includes: substrate; An inorganic coating is disposed on the surface of the substrate; The inorganic coating comprises a silicon oxide network structure; The nano titanium oxide coating is arranged on the surface of the inorganic coating.

2. The long-lasting photocatalyst coating according to claim 1, characterized in that: The thickness of the nano titanium oxide coating is ≤100nm; the particle size of the nano titanium oxide particles in the nano titanium oxide coating is 5-100nm.

3. The long-lasting photocatalyst coating according to claim 2, characterized in that: The thickness of the nano titanium oxide coating is ≤50nm; the particle size of the nano titanium oxide particles in the nano titanium oxide coating is 5-50nm.

4. The long-lasting photocatalyst coating according to claim 1, characterized in that: The raw materials of the coating for forming the inorganic coating include: 39-59wt% of organic alkoxysilane, 39-59wt% of silica sol, and 0.5-2wt% of functional additive; the total amount of the organic alkoxysilane, silica sol and functional additive is 100%; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, and m is a natural number from 0 to 3.

5. The long-lasting photocatalyst coating according to claim 1, characterized in that: The raw materials of the coating for forming the inorganic coating include: 70-80wt% of solution; 5-10wt% of functional additives, wherein the functional additives are selected from potassium titanate, aluminum oxide or a combination of the two; 10-20wt% of inorganic pigments; 0.5-2.0wt% of other functional additives; the raw materials of the solution include the following components: 30-40wt% of organic alkoxysilane, 15-20wt% of organic solvent, and 25-30wt% of silica sol; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, m is a natural number from 0 to 3; the above percentages are the mass percentages of each raw material in the total weight of the inorganic coating.

6. The long-lasting photocatalyst coating according to claim 1, characterized in that: The raw materials of the coating for forming the inorganic coating include: 30-99.9% inorganic resin; 0.1-70% silicon nitride; 0-10% functional additives; 0-18% inorganic pigments; 0-2% other functional additives; the total amount of the coating is 100%; wherein the inorganic resin is obtained by mixing and reacting an organic alkoxysilane, an organic solvent and a silica sol, extracting alcohol, and adding deionized water; the mass ratio of the organic alkoxysilane, the organic solvent and the silica sol is 1-1.6:0.5-0.8:1; the organic alkoxysilane has a molecular formula R 1 m Si(OR 2 ) 4-m Indicates; the R 1 is selected from alkyl; said R 2 is selected from an alkyl group; the general formula of the alkyl group is C n H 2n+1 , wherein n is a positive integer from 1 to 10; the R 1 and the OR 2 The total number is 4, and m is a natural number of 0 to 3; the inorganic resin is an acidic cationic system; the VOC content of the inorganic resin is ≤10% by mass percentage; and the functional additive is selected from at least one of potassium titanate, aluminum oxide and nano-silicon oxide.

7. The long-lasting photocatalyst coating according to claim 1, characterized in that: The coating material forming the nano titanium oxide coating is a water and / or alcohol dispersion of nano titanium oxide.

8. A method for preparing a long-lasting photocatalyst coating, characterized in that: It includes the following steps: S11: placing an inorganic coating on the surface of the substrate; S12: when the inorganic coating is in a wet state, a nano titanium oxide coating is provided on the surface of the inorganic coating; the nano titanium oxide coating is a water and / or alcohol dispersion of nano titanium oxide; S13 nano titanium oxide coating is fused with inorganic coating and dried to obtain a long-lasting photocatalyst coating.

9. The preparation method according to claim 8, characterized in that: The inorganic coating being in a wet state refers to a state in which the inorganic coating has not yet dried on the surface.

10. Use of the long-acting photocatalyst coating according to any one of claims 1 to 7 in the field of sterilization or self-cleaning.

Citation Information

Patent Citations

  • Transparent titania super-hydrophilic coating using organosilicon as underlayment and preparation thereof

    CN101205121A

  • Room-temperature curable inorganic coating and manufacturing method thereof

    CN105038335A

  • Mesh-shaped titanium dioxide photocatalyst material, preparation method and application thereof, and equipment

    CN115770562A

  • Method for carrying photo-catalyst particle

    JP1997271676A

  • Formation of photocatalyst film on organic substrate and its use

    JP1999319709A