Copper foil warping reducing agent and preparation method thereof
By using warpage reducing agents containing N-(3-sulfopropyl)-saccharin sodium, polypropylene glycol, gelatin and fatty amine ethoxysulfonates in the production of electrolytic copper foil, adsorbing on the crystal surface of the preferred orientation adsorption surface, The warping problem caused by compressive stress imbalance of electrolytic copper foil is solved, the tensile strength and elongation of the copper foil are improved, and the degree of warping is reduced.
Patent Information
- Application Number
- CN202411026315.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
During the production process, electrolytic copper foil is prone to warping due to compressive stress imbalance, resulting in serious warping, affecting production efficiency and quality.
A copper foil warpage reducing agent is used, containing N-(3-sulfopropyl)-saccharin sodium, polypropylene glycol, gelatin and fatty amine ethoxysulfonate, which is reduced by adsorption on the crystal surface of the preferred orientation adsorption surface. Growth speed, pull the growth rate between the preferred orientation adsorption surface and other crystal surfaces, increase the proportion of twin boundaries, release internal stress, and reduce the residual stress of electrolytic copper foil.
It effectively reduces the warping degree of electrolytic copper foil, improves the tensile strength and elongation of the copper foil, stabilizes the plane direction performance of the copper foil, and reduces the warping problem.
Smart Images

Figure CN118957686A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a copper foil warpage reducing agent and a preparation method thereof, and belongs to the technical field of copper foil production. Background Art
[0002] At present, electrolytic copper foil is an important material for copper clad laminate (CCL), printed circuit board (PCB), and lithium-ion battery manufacturing. As the modern electronic industry has entered a stage of rapid development, the status of high-quality electrolytic copper foil with good stability has also been significantly improved. However, in the actual production process of electrolytic copper foil, due to the types of additives used, the morphology of the cathode roller surface, the stress when the copper foil is peeled off from the cathode roller, and impurities during surface treatment, etc., the peeled copper foil will warp. Severely warped copper foil is prone to dislocation and wrinkles during the production process.
[0003] The warping of electrolytic copper foil is caused by the imbalance of compressive stress on both sides of the copper foil. When the copper foil warps and deforms, a large amount of internal stress is not released, thus forming a macroscopic residual stress of the entire copper foil. The greater the residual stress, the more serious the warping.
[0004] The mechanism of internal stress formation in copper foil is very complex, and is affected by a series of factors such as the surface morphology of the cathode roller, impurities, and process parameters. These factors can cause the copper ions to be misaligned and slip during the electrodeposition process, leading to the formation of twins and twin boundaries. The arrangement of copper atoms deviates from the structural area of the ideal crystal, destroying the symmetry of the entire crystal, thereby generating internal stress. And because there are gaps between particles on the rough surface, the compressive stress on the rough surface is easier to release than on the smooth surface, which makes the compressive stress on the smooth surface greater than that on the rough surface, so the copper foil is bent with the smooth surface facing the rough surface as a whole.
[0005] In view of the above-mentioned defects, the present invention aims to create a copper foil warpage reducing agent and a preparation method thereof, so as to make it more valuable for industrial use. Summary of the invention
[0006] In order to solve the above technical problems, the purpose of the present invention is to provide a copper foil warpage reducing agent and a preparation method thereof.
[0007] A copper foil warpage reducing agent of the present invention, wherein each aqueous solution of the warpage reducing agent contains:
[0008] 95-105 g N-(3-sulfopropyl)-saccharin sodium;
[0009] 35-45g polypropylene glycol;
[0010] 0.7-0.8 g gelatin;
[0011] 0.15-0.25g fatty amine ethoxy sulfonate. The anti-warping agent of the present invention is adsorbed on the preferred orientation adsorption surface crystal plane, reducing its growth rate, pulling the growth rate between the preferred orientation adsorption surface crystal plane and other crystal planes, thereby retaining the preferred orientation adsorption surface crystal plane parallel to the substrate, promoting the formation of the preferred orientation adsorption surface texture, so that no preferred crystal orientation appears on the copper foil surface, ensuring the stability of the tensile strength and elongation of the copper foil along the plane direction; increasing the twin boundary ratio, thereby increasing the release of the internal stress of the copper foil, thereby reducing the residual stress of the electrolytic copper foil, and finally reducing the warping of the electrolytic copper foil.
[0012] Furthermore, the molecular weight of the polypropylene glycol is 400-6000.
[0013] Furthermore, the solvent of the copper foil warpage reducing agent is deionized water.
[0014] Further, the specific preparation steps are:
[0015] N-(3-sulfopropyl)-saccharin sodium, polypropylene glycol, gelatin, fatty amine ethoxy sulfonate and deionized water are mixed according to a proportion, and the mixture is stirred and evenly mixed to prepare a copper foil warpage reducing agent.
[0016] A method for applying a copper foil warpage reducing agent, wherein the specific application steps are as follows:
[0017] (1) The electrolyte is prepared according to the following ratio: 320-340 g / L of copper sulfate pentahydrate, 95-105 g / L of concentrated sulfuric acid, 18-22 mg / L of chloride ions, and the solvent is deionized water; the anti-warping agent of the present invention can be adsorbed on the surface of the cathode under the synergistic effect of chloride ions, thereby forming a dense polymer film. It is difficult to obtain a copper foil with stable performance when Cl- is added to the electrolyte alone, and it is also necessary to synergize with the anti-warping agent of the present invention. When the anti-warping agent is added, the chloride ions will interact with the anti-warping agent to form a more complex complex to achieve super co-electrodeposition, thereby affecting the roughness, tensile strength, elongation, yield strength and other mechanical properties of the electrolytic copper foil. And because this dense polymer film will not enter the deposited copper layer in large quantities during the electroplating process, but instead maintains an adsorption-desorption process of desorption from the old copper layer and then adsorption on the new copper layer, the dense polymer film can be continuously adsorbed on the surface of the newly deposited copper layer. Since the mean free path of diffusion of the adsorbed ion layer is reduced when there are adsorbed additives in the plating solution, this dense polymer film can act as a diffusion barrier to limit the diffusion of copper ions, thereby reducing the deposition rate of copper ions on the cathode plate surface. At the same time, the difference between the high current area and the low current area is reduced, so that copper ions can be deposited evenly on the cathode. In this way, the surface tension of the interface can be reduced by reducing the contact angle. The purpose of promoting the preferential orientation of the adsorption surface texture is achieved, or the purpose of refining the copper foil grains is achieved to affect the internal stress of the copper foil, thereby affecting the degree of warping of the copper foil.
[0018] (2) during the copper electroplating process, 0.5 to 2.5 L of the copper foil warpage reducing agent is added per cubic meter of copper plating electrolyte for electroplating;
[0019] (3) Baking is performed after the electrolysis is completed. The anti-warping agent of the present invention causes the preferred orientation of the preferred orientation adsorption surface crystal plane to show a downward trend at the microscopic level, thereby increasing the growth rate between the preferred orientation adsorption surface crystal plane and other crystal planes, promoting the formation of the preferred orientation adsorption surface texture, achieving the purpose of balancing the internal stress of the electrolytic copper foil and reducing the residual stress of the electrolytic copper foil, thereby reducing the warping of the electrolytic copper foil.
[0020] Compared with the electrolytic copper foil anti-warping agent prepared by the present invention, the release of the internal stress of the copper foil is also increased due to the increase in the proportion of twin boundaries, thereby reducing the residual stress of the electrolytic copper foil and ultimately reducing the warping of the electrolytic copper foil.
[0021] Furthermore, the electroplating temperature is 52-55° C., the current density is 60 A / dm 2 , and the time is 40 s.
[0022] Furthermore, the oven temperature is 135-145° C., and the baking time is 15 minutes.
[0023] By means of the above scheme, the present invention has at least the following advantages:
[0024] The anti-warping agent of the present invention can be adsorbed on the surface of the cathode under the synergistic effect of chloride ions, thereby forming a dense polymer film. It is difficult to obtain a copper foil with stable performance when Cl- is added alone in the electrolyte, and it is also necessary to synergize with the anti-warping agent of the present invention. When the anti-warping agent is added, the chloride ions will interact with the anti-warping agent to form a more complex complex to achieve super co-electrodeposition, thereby affecting the roughness, tensile strength, elongation, yield strength and other mechanical properties of the electrolytic copper foil. And because this dense polymer film will not enter the deposited copper layer in large quantities during the electroplating process, it will maintain an adsorption-desorption process of desorbing from the old copper layer and then adsorbing on the new copper layer, so that this dense polymer film can be continuously adsorbed on the surface of the newly deposited copper layer. Since there is an adsorbed additive in the plating solution, the mean free path of the diffusion of the adsorbed ion layer is reduced, so this dense polymer film can be used as a diffusion barrier to limit the diffusion of copper ions, thereby achieving the effect of reducing the deposition rate of copper ions on the cathode plate surface. At the same time, the difference between the high current area and the low current area is reduced, so that copper ions can be uniformly deposited on the cathode. In this way, the surface tension of the interface can be reduced by reducing the contact angle, so as to promote the preferred orientation adsorption surface texture, or refine the copper foil grains to affect the internal stress of the copper foil, and then affect the degree of copper foil warping.
[0025] The anti-warping agent of the present invention is adsorbed on the crystal plane of the preferential orientation adsorption surface, reduces its growth rate, and increases the growth rate between the crystal plane of the preferential orientation adsorption surface and other crystal planes, thereby retaining the crystal plane of the preferential orientation adsorption surface parallel to the substrate, promoting the formation of the texture of the preferential orientation adsorption surface, so that no preferential crystal orientation appears on the surface of the copper foil, ensuring the stability of the tensile strength and elongation of the copper foil along the plane direction; increasing the proportion of twin boundaries, thereby increasing the release of stress in the copper foil, thereby reducing the residual stress of the electrolytic copper foil, and finally reducing the warping of the electrolytic copper foil.
[0026] The anti-warping agent of the present invention causes the preferred orientation of the preferred orientation adsorption surface crystal plane to show a downward trend at the microscopic level, thereby increasing the growth rate between the preferred orientation adsorption surface crystal plane and other crystal planes, promoting the formation of the preferred orientation adsorption surface texture, achieving the purpose of balancing the internal stress of the electrolytic copper foil, reducing the residual stress of the electrolytic copper foil, and thus reducing the warping of the electrolytic copper foil.
[0027] Compared with the electrolytic copper foil anti-warping agent prepared by the present invention, the release of the internal stress of the copper foil is also increased due to the increase in the proportion of twin boundaries, thereby reducing the residual stress of the electrolytic copper foil and ultimately reducing the warping of the electrolytic copper foil.
[0028] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show a certain embodiment of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 is the XRD diagram after the warpage reducing agent of the present invention is added;
[0031] Figure 2 is the grain orientation diagram before the warpage reducing agent of the present invention is added;
[0032] Figure 3 It is the grain orientation diagram after the warpage reducing agent of the present invention is added. DETAILED DESCRIPTION
[0033] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0034] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains:
[0035] 95-105 g N-(3-sulfopropyl)-saccharin sodium;
[0036] 35-45g polypropylene glycol;
[0037] 0.7-0.8 g gelatin;
[0038] 0.15-0.25 g fatty amine ethoxylate;
[0039] The molecular weight of the polypropylene glycol is 400-6000;
[0040] The solvent of the copper foil warpage reducing agent is deionized water;
[0041] The preparation steps of the copper foil warpage reducing agent are as follows: N-(3-sulfopropyl)-saccharin sodium, polypropylene glycol, gelatin, fatty amine ethoxy sulfonate and deionized water are mixed according to a ratio, and the mixture is stirred and mixed to obtain the copper foil warpage reducing agent;
[0042] Application method of the copper foil warpage reducing agent:
[0043] Prepare the electrolyte according to the following ratio: 320-340 g / L of copper sulfate pentahydrate, 95-105 g / L of concentrated sulfuric acid, 18-22 mg / L of chloride ions, and the rest is deionized water;
[0044] In the copper electroplating process, 0.5 to 2.5 L of the copper foil warpage reducing agent is added to each cubic meter of copper plating electrolyte for electroplating. The electroplating temperature is 52 to 55°C and the current density is 60A / dm 2 , time is 40s.
[0045] After the electrolysis is completed, baking is carried out, the oven temperature is 135-145°C, and the baking time is 15 minutes.
[0046] Embodiment 1:
[0047] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains: 95g of N-(3-sulfopropyl)-saccharin sodium, 35g of polypropylene glycol, 0.7g of gelatin, and 0.15g of fatty amine ethoxy sulfonate.
[0048] In the copper electroplating process, 0.5 L of the warpage reducing agent prepared in this embodiment is added to each cubic meter of copper plating electrolyte for electroplating. The electrolyte contains: 320 g / L of copper sulfate pentahydrate, 95 g / L of concentrated sulfuric acid, 18 mg / L of chloride ions, the temperature is 52° C., and the current density is 60 A / dm 2 The baking time is 40 seconds. The oven temperature is 135°C and the baking time is 15 minutes.
[0049] Embodiment 2:
[0050] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains: 98g of N-(3-sulfopropyl)-saccharin sodium, 38g of polypropylene glycol, 0.73g of gelatin, and 0.18g of fatty amine ethoxy sulfonate.
[0051] In the copper electroplating process, 1 L of the warpage reducing agent prepared in this embodiment is added to each cubic meter of copper plating electrolyte for electroplating. The electrolyte contains: 325 g / L of copper sulfate pentahydrate, 98 g / L of concentrated sulfuric acid, 19 mg / L of chloride ions, the temperature is 53° C., the current density is 60 A / dm2, and the time is 40 s. The oven temperature is 140° C. and the baking time is 15 min.
[0052] Embodiment 3:
[0053] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains: 100g of N-(3-sulfopropyl)-saccharin sodium, 40g of polypropylene glycol, 0.75g of gelatin, and 0.2g of fatty amine ethoxy sulfonate.
[0054] In the copper electroplating process, 1.5 L of the warpage reducing agent prepared in this embodiment is added to each cubic meter of copper plating electrolyte for electroplating. The electrolyte contains: 330 g / L of copper sulfate pentahydrate, 100 g / L of concentrated sulfuric acid, 20 mg / L of chloride ions, the temperature is 54° C., the current density is 60 A / dm2, and the time is 40 s. The oven temperature is 140° C. and the baking time is 15 min.
[0055] Embodiment 4:
[0056] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains: 103g of N-(3-sulfopropyl)-saccharin sodium, 43g of polypropylene glycol, 0.78g of gelatin, and 0.22g of fatty amine ethoxy sulfonate.
[0057] During the copper electroplating process, 2 L of the warpage reducing agent prepared in this embodiment was added to each cubic meter of copper plating electrolyte for electroplating. The electrolyte contained: 335 g / L of copper sulfate pentahydrate, 103 g / L of concentrated sulfuric acid, 21 mg / L of chloride ions, the temperature was 55° C., the current density was 60 A / dm2, and the time was 40 s. The oven temperature was 140° C. and the baking time was 15 min.
[0058] Embodiment 5:
[0059] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains: 105g of N-(3-sulfopropyl)-saccharin sodium, 45g of polypropylene glycol, 0.8g of gelatin, and 0.25g of fatty amine ethoxy sulfonate.
[0060] During the copper electroplating process, 2.5 L of the warpage reducing agent prepared in this embodiment was added to each cubic meter of copper plating electrolyte for electroplating. The electrolyte contained: 340 g / L of copper sulfate pentahydrate, 105 g / L of concentrated sulfuric acid, 22 mg / L of chloride ions, the temperature was 55° C., the current density was 60 A / dm2, and the time was 40 s. The oven temperature was 140° C. and the baking time was 15 min.
[0061] Comparative Example 1:
[0062] The warpage reducing agent of the present invention is not used in the copper electroplating process, the electrolyte contains: 330 g / L of copper sulfate pentahydrate, 100 g / L of concentrated sulfuric acid, 20 mg / L of chloride ions, the temperature is 55°C, the current density is 60 A / dm2, the time is 40 s, the oven temperature is 140°C, and the baking time is 15 min.
[0063] Comparative Example 2:
[0064] A copper foil warpage reducing agent, wherein each aqueous solution of the warpage reducing agent contains: 100g of N-(3-sulfopropyl)-saccharin sodium, 40g of polypropylene glycol, 0.75g of gelatin, and 0.2g of fatty amine ethoxy sulfonate.
[0065] In the copper electroplating process, 1.5 L of the warpage reducing agent prepared in this embodiment is added to each cubic meter of copper plating electrolyte for electroplating. The electrolyte contains: 330 g / L of copper sulfate pentahydrate, 100 g / L of concentrated sulfuric acid, the temperature is 55° C., the current density is 60 A / dm2, and the time is 40 s. The oven temperature is 140° C. and the baking time is 15 min.
[0066] The samples of Examples 1-5 and Comparative Examples 1-2 were placed in a dry and windless environment, and their warping conditions were compared, and their physical properties were tested. The test results are shown in Table 1:
[0067] Testing method: Place the prepared copper foil in an oven and bake at 140℃ for 15 minutes. After baking, cut the foil into strips with a length of 50mm and a width of 12.8mm. Use an electronic universal testing machine to test its tensile strength and elongation: Place the sample vertically into the tensile strength test fixture, set the speed of the tensile machine to 50.8mm / min, the distance between the chucks to 50mm, and then break the sample. Calculate the tensile strength and elongation of the copper foil according to the following formula.
[0068] Tensile strength test: Copper foil tensile strength (MPa) = maximum tensile force (N) / average cross-sectional area (mm2) Elongation test: Elongation (%) = (length after stretching - original standard length) / original standard length * 100% Warping degree test: Place the copper foil at room temperature on a horizontal table and use a measuring ruler to measure the warping.
[0069] Table 1 Performance test results
[0070]
[0071] From Table 1 and Figure 1-Figure 3 It can be seen that compared with Comparative Example 1, in Examples 1-5, the copper foil warpage reducing agent of the present invention is added to the copper plating electrolyte. As the amount of the copper foil added increases, the warpage of the copper foil gradually decreases, and the tensile and elongation properties of the copper foil are significantly improved; it is fully proved that the warpage reducing agent of the present invention can be adsorbed on the crystal plane of the preferentially oriented adsorption surface, reduce its growth rate, and separate the growth rate between the crystal plane of the preferentially oriented adsorption surface and other crystal planes, thereby retaining the crystal plane of the preferentially oriented adsorption surface parallel to the substrate, and promoting the formation of the texture of the preferentially oriented adsorption surface, so that no preferential crystal orientation appears on the surface of the copper foil, ensuring the stability of the tensile strength and elongation of the copper foil along the plane direction; increasing the proportion of twin boundaries, thereby increasing the release of stress inside the copper foil, thereby reducing the residual stress of the electrolytic copper foil, and ultimately reducing the warpage of the electrolytic copper foil.
[0072] Comparing Example 3 with Comparative Example 2, since no chloride ions are added to the electrolyte in Comparative Example 2, the warping degree of the final copper foil is increased. It can be confirmed that the present invention can be adsorbed on the surface of the cathode under the synergistic effect of chloride ions, thereby forming a dense polymer film, and since this dense polymer film will not enter the deposited copper layer in large quantities during the electroplating process, it maintains an adsorption-desorption process of desorption from the old copper layer and then adsorption on the new copper layer, so that this dense polymer film can be continuously adsorbed on the surface of the newly deposited copper layer. Since the adsorbed additive exists in the plating solution, the mean free path of the diffusion of the adsorbed ion layer is reduced, so this dense polymer film can be used as a diffusion barrier to limit the diffusion of copper ions, thereby achieving the effect of reducing the deposition rate of copper ions on the cathode plate surface. At the same time, the difference between the high current area and the low current area is reduced, so that copper ions can be uniformly deposited on the cathode. In this way, the surface tension of the interface can be reduced by reducing the contact angle. The purpose of promoting the preferred orientation adsorption surface texture preference, or refining the copper foil grains to affect the internal stress of the copper foil, and then the degree of warping of the copper foil is affected.
[0073] There is no Cl- in the copper foil bath solution, the copper foil is poorly leveled, the crystals are rough with pinholes and burrs, it is easy to burn and difficult to peel off.
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A copper foil warpage reducing agent, characterized in that: Each aqueous solution of the warpage reducer contains: 95-105 g N-(3-sulfopropyl)-saccharin sodium; 35-45g polypropylene glycol; 0.7-0.8 g gelatin; 0.15-0.25 g fatty amine ethoxylate.
2. The copper foil warpage reducing agent according to claim 1, characterized in that: The molecular weight of the polypropylene glycol is 400-6000.
3. The copper foil warpage reducing agent according to claim 1, characterized in that: The solvent of the copper foil warpage reducing agent is deionized water.
4. The method for preparing a copper foil warpage reducing agent according to claim 1, characterized in that: The specific preparation steps are: N-(3-sulfopropyl)-saccharin sodium, polypropylene glycol, gelatin, fatty amine ethoxy sulfonate and deionized water are mixed according to a proportion, and the mixture is stirred and evenly mixed to prepare a copper foil warpage reducing agent.
5. The method for applying the copper foil warpage reducing agent according to any one of claims 1 to 4, characterized in that: The specific application steps are: (1) preparing an electrolyte according to the following ratio: 320-340 g / L of copper sulfate pentahydrate, 95-105 g / L of concentrated sulfuric acid, 18-22 mg / L of chloride ions, and deionized water as the solvent; (2) during the copper electroplating process, 0.5 to 2.5 L of the copper foil warpage reducing agent is added per cubic meter of copper plating electrolyte for electroplating; (3) Baking is performed after the electrolysis is completed.
6. The application method of the copper foil warpage reducing agent according to claim 5, characterized in that: The electroplating temperature is 52-55° C., the current density is 60 A / dm 2 , and the time is 40 s.
7. The application method of the copper foil warpage reducing agent according to claim 5, characterized in that: The oven temperature is 135-145° C., and the baking time is 15 minutes.
Citation Information
Cited By
Preparation method of electrolytic copper foil with low internal stress
CN121593139A
A composite electrolyte for low-stress lithium battery copper foil and a method for preparing low-stress lithium battery copper foil
CN122918656A