Breathable coating material and application thereof in earthen archaeological site protection

By using air permeable coating materials formed by chloroethylene aqueous fluorine, aluminosilicate, straw and dispersant, the problem of poor permeability in the prior art is solved, and the effective substances and gases inside and outside the site in the protection of soil sites are achieved. Exchange provides better protection.

CN118909474AActive Publication Date: 2024-11-08SHAANXI NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410960780.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The materials used in the existing chemical reinforcement method for soil site protection have poor permeability and are prone to blockage of pores, which is not conducive to the exchange of substances and gases inside and outside the site.

Method used

The breathable coating material formed by chloroethylene aqueous fluorine, aluminosilicate, straw and dispersant is waterproof but not water-repellent, has good breathability, and is suitable for soil site protection.

Benefits of technology

The breathable coating material does not clog the pores, which is conducive to the exchange of substances and gases inside and outside the site, provides better protection effects, and maintains the weather resistance and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909474A_ABST
    Figure CN118909474A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of coating materials, and particularly relates to a breathable coating material and application thereof in earthen archaeological site protection, the breathable coating material comprises chlorotrifluoroethylene water-based fluorine, aluminosilicate, straw, a dispersing agent and water, the mass ratio of the chlorotrifluoroethylene water-based fluorine to the aluminosilicate to the straw to the water is (5-15): (1-5): (1-5): (75-95), the volume of the dispersing agent corresponding to every 10 g of trifluorochloroethylene water-based fluorine is 1-2 ml. The breathable coating material disclosed by the invention is waterproof but not water-repellent, has good breathability, does not block air holes, is beneficial to exchange between substances and gas inside and outside a ruin, and has a good protection effect on the earthen ruin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coating materials, and in particular relates to a breathable coating material and an application thereof in the protection of earthen ruins. Background Art

[0002] The protection of earthen sites is one of the recognized problems in the field of cultural relics protection in the world. At present, earthen sites are affected by natural environment or human destruction to varying degrees, among which weathering is one of the leading causes of destruction. Scholar Li Tonglin disclosed in his master's thesis "Research on the Reinforcement Methods of Earthen Sites and Their Seismic Stability" that there are three methods for the protection of earthen sites from weathering: backfill protection, physical reinforcement and chemical reinforcement. The backfill protection method is a temporary rescue protection method for construction projects, with temporary burial as the main purpose; the physical reinforcement method includes anchor reinforcement and support method, which are applied to severely cracked earthen sites, but are not suitable for the weathering protection of most earthen sites; the chemical reinforcement method is to use chemical reinforcement materials to improve the surface rock and soil, increase the cohesion and hardness of the site soil, and thus increase the weathering resistance of the site itself. Compared with the above two reinforcement methods, it can achieve the purpose of long-term protection of earthen sites while following the principle of "repairing the old as the old" for cultural relics, and has more obvious protection advantages.

[0003] At present, the reinforcement materials used in chemical reinforcement methods can be divided into two categories: inorganic protective materials and organic protective materials. Inorganic reinforcement materials mainly include lime water, water glass, barium hydroxide, etc. Inorganic materials have good compatibility with inorganic cultural relics, but because their reinforcement mechanism is based on the chemical reaction between the reinforcement material and the site matrix, the reactants can easily block the pores on the surface of the site and prevent the penetration of the reinforcement agent, resulting in shallow penetration depth, poor cohesion between the reinforcement material and the site, and weak reinforcement effect. Organic materials include polymer materials such as acrylates and organic fluorines. Acrylic materials have strong adhesion, good permeability and film-forming properties, but there is a migration phenomenon in the reinforced material. After reinforcement, the aging resistance is poor, and the surface is prone to yellowing, whitening and discoloration; organic fluorine materials have good aging resistance, chemical corrosion resistance, oxidation resistance and excellent mechanical properties, but because they carry a -CF3 group, they are highly hydrophobic. Current studies have found that hydrophobic polymer materials can cause moisture expansion stress between interfaces and damage cultural relics; for example, through the study of the hydrophobicity, stability, and permeability of gases such as O2, N2, and CO2 of fluorine-containing polymer materials, it was found that fluorine-containing polymer materials have poor gas permeability and poor air permeability. When this material is used for site protection, it is easy to block the pores, which is not conducive to the exchange of substances and gases inside and outside the site. Summary of the invention

[0004] In view of the technical problem that existing protective materials have poor permeability, easily clog pores, and are not conducive to the exchange of substances and gases inside and outside the site, the present invention provides a breathable coating material and its application in the protection of earthen sites.

[0005] The present invention adopts trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and dispersant to form a breathable coating material, which is waterproof but not water-repellent, has good air permeability, does not block pores, is conducive to the exchange of substances and gases inside and outside the ruins, and has a good protective effect on the earthen ruins.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A breathable coating material comprises trifluorochloroethylene aqueous fluorine, aluminosilicate, straw, a dispersant and water, wherein the mass ratio of trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and water is 5-15:1-5:1-5:75-95, and the volume of the dispersant corresponding to every 10g of trifluorochloroethylene aqueous fluorine is 1ml-2ml.

[0008] It is further defined that the mass ratio of trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and water is 10:2.5:2.5:85, and the volume of the dispersant corresponding to every 10g of trifluorochloroethylene aqueous fluorine is 1.5ml.

[0009] It is further defined that the straw is corn straw, rice straw or wheat straw; the dispersant is Tween-80, octylphenol polyoxyethylene ether, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate; and the aluminosilicate is sodium aluminosilicate, potassium aluminosilicate or calcium aluminosilicate.

[0010] It is further defined that the breathable coating material has an average air permeability coefficient of 0.00586 g / (25 cm 2 h).

[0011] It is further defined that the breathable coating material has a water absorption rate of 16.9% and a contact angle of 75.5°.

[0012] A method for preparing the breathable coating material comprises the following steps:

[0013] S1. Take trifluorochloroethylene aqueous fluorine, aluminosilicate, straw, dispersant and water according to the mass parts;

[0014] S2, washing and drying the straw, crushing and sieving after drying to obtain straw powder;

[0015] S3, mixing aqueous fluorine of chlorotrifluoroethylene, aluminosilicate, water and the straw powder of step S2, adding a dispersant, stirring evenly, and obtaining a breathable coating material.

[0016] It is further defined that in step S2, the drying temperature is 75° C. to 85° C., the drying time is 24 h to 48 h, and the particle size of the straw powder is 80 mesh to 120 mesh.

[0017] It is further defined that in step S3, the stirring conditions are: temperature 30°C to 40°C, stirring speed 600r / min to 1000r / min, and stirring time 1.5h to 2.5h.

[0018] The application of the breathable coating material in the protection of earthen ruins.

[0019] It is further defined that the application is to apply the breathable coating material as a coating on the inner walls of the earthen ruins.

[0020] The beneficial effects of the present invention are:

[0021] 1. The present invention adopts trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and dispersant to form a breathable coating material, which is waterproof but not water-repellent, has good air permeability, does not block pores, is conducive to the exchange of substances and gases inside and outside the ruins, and plays a good protective role on the earthen ruins.

[0022] 2. In the present invention, straw is used to modify trifluorochloroethylene water-based fluorine. On the one hand, the straw destroys the original dense structure of the water-based fluorine, making it loose and generating pores, which greatly improves the air permeability of the coating. On the other hand, the straw powder itself contains lignin. After high-temperature treatment, part of the lignin is thermally cracked, and small molecular gases are discharged to leave pores, which further improves the air permeability of the coating.

[0023] 3. Adding a dispersant to the coating material of the present invention can, on the one hand, play a dispersing role, thereby improving the uniformity, leveling and film-forming properties of the material; on the other hand, it can also play a surfactant role, thereby reducing the surface tension of the coating material, thereby improving its hydrophilicity, and increasing the air permeability and water permeability of the cultural relics without affecting the material and energy exchange capacity of the cultural relics themselves.

[0024] 4. The present invention selects trifluorochloroethylene water-based fluorine as the basic material, and modifies it by adding straw, dispersant and aluminosilicate, etc., while retaining the excellent weather resistance and mechanical properties of trifluorochloroethylene water-based fluorine, it can slightly reduce the hydrophobicity of the material and increase its water permeability, so that the material has waterproof but not water-repellent properties; in addition, the modified coating material also has good anti-aging properties, achieving the effect of protecting cultural relics from long-term discoloration and not changing the original historical appearance.

[0025] 5. The raw materials selected in the present invention are easily available, the preparation method is simple, and industrial production can be realized. The formed coating material has broad application prospects in the protection of earthen sites, especially the protection of revolutionary sites. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Photos of films formed from three different coating materials;

[0027] Figure 2 Infrared spectra of films formed from three different coating materials;

[0028] Figure 3 The microscopic morphology of the cross section of the coating 1 film at 50 μm and 25 μm;

[0029] Figure 4 The microscopic morphology of the cross section of coating 2 film at 50 μm and 25 μm;

[0030] Figure 5 The microscopic morphology of the cross section of coating 3 film at 50μm and 25μm;

[0031] Figure 6 The air permeability test of samples treated with three different coatings under the same conditions;

[0032] Figure 7 Contact angle test of samples treated with different coatings;

[0033] Figure 8 Dry heat aging test of samples treated with three different coatings and untreated samples;

[0034] Fig. 9 It is a wet heat aging test of samples treated with three different coatings and untreated samples;

[0035] Fig.10 Freeze-thaw aging test of samples treated with three different coatings and untreated samples. DETAILED DESCRIPTION

[0036] The technical solution protected by the present invention is now described in detail in conjunction with the accompanying drawings and embodiments. However, it is obvious that the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the described embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0037] The invention provides a breathable coating material, which comprises trifluorochloroethylene aqueous fluorine, aluminosilicate, straw, a dispersant and water.

[0038] In the present invention, the mass ratio of trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and water is 5-15:1-5:1-5:75-95, and the volume of the dispersant corresponding to 10g of trifluorochloroethylene aqueous fluorine is 1ml-2ml.

[0039] In the present invention, the mass ratio of aqueous fluorine of chlorotrifluoroethylene, aluminosilicate, straw and water can be 5:1:1:75, 15:5:5:95 (3:1:1:19); 15:1:1:75, 15:1:1:95, 5:1:5:75, 10:1:1:75, 10:5:5:75 (5:1:1:25), 10:1:1:95, 10:2.5:2.5:75 or 10:2.5:2.5:95, and can also be other mass ratios within the specified range.

[0040] In the present invention, the volume of the dispersant corresponding to each 10g of trifluorochloroethylene aqueous fluorine is 1ml, 1.2ml, 1.5ml, 1.8ml or 2ml.

[0041] Preferably, the mass ratio of trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and water is 10:2.5:2.5:85, and the volume of the dispersant corresponding to every 10g of trifluorochloroethylene aqueous fluorine is 1.5ml.

[0042] In the present invention, the straw is corn straw, rice straw or wheat straw, and may also be other crop straw or other plant branches containing lignin.

[0043] In the present invention, the aluminosilicate may be sodium aluminosilicate, potassium aluminosilicate or calcium aluminosilicate.

[0044] In the present invention, the dispersant is Tween-80, octylphenol polyoxyethylene ether, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate.

[0045] The method for preparing the breathable coating material provided by the present invention comprises the following steps:

[0046] S1. Take trifluorochloroethylene aqueous fluorine, aluminosilicate, straw, dispersant and water according to the mass parts.

[0047] S2, washing and drying the straw, crushing and sieving after drying to obtain straw powder.

[0048] In step S2 of the present invention, the drying temperature is 75° C. to 85° C., the drying time is 24 h to 48 h, and the particle size of the straw powder is 80 meshes to 120 meshes.

[0049] In the present invention, the drying temperature is 75°C, 80°C or 85°C, the drying time is 24h, 28h, 30h, 32h, 36h, 40h, 42h, 45h or 48h, and the particle size of the straw powder is 80 mesh, 90 mesh, 100 mesh, 110 mesh or 120 mesh.

[0050] S3, mixing aqueous fluorine of chlorotrifluoroethylene, aluminosilicate, water and the straw powder of step S2, adding a dispersant, stirring evenly, and obtaining a breathable coating material.

[0051] In the present invention, the stirring conditions are: stirring temperature 30° C. to 40° C., stirring speed 600 r / min to 1000 r / min, and stirring time 1.5 h to 2.5 h.

[0052] In the present invention, the stirring temperature is 30°C, 32°C, 35°C, 38°C or 40°C, the stirring speed is 600r / min, 700r / min, 800r / min, 900r / min or 1000r / min, and the stirring time is 1.5h, 2.0h or 2.5h.

[0053] The air-permeable coating material obtained by the invention has excellent air permeability, water permeability and anti-aging performance, and can be used as a protective material in the protection of earthen ruins.

[0054] The present invention is described in detail below with reference to specific embodiments.

[0055] It should be noted that, unless otherwise specified, the reagents and drugs used in the following examples and experiments are conventional commercially available products.

[0056] It should be noted that, unless otherwise specified, the operations used in the following examples and experiments are routine operations in the art.

[0057] In the following examples, the experimental materials used are as follows.

[0058] Chlorotrifluoroethylene water-based fluorine, Dalian Zhenbang Fluorine Coating Co., Ltd.; dispersant is octylphenol polyoxyethylene ether, Tianjin Fuyu Fine Chemical Co., Ltd.; anhydrous sodium sulfate, Tianjin Dingshengxin Chemical Co., Ltd.; sodium aluminosilicate, Anhui Zesheng Technology Co., Ltd.; ultrapure water.

[0059] In the following examples, the experimental instruments used are shown in Table 1.

[0060] Table 1 Experimental instruments

[0061] Instrument Name model Manufacturer Colorimeter X-Rite VS-450 X-Rite Instruments, Inc. High power CNC ultrasonic cleaner KQ-800KDE Kunshan Ultrasonic Instrument Co., Ltd. Electronic balance HX3002T Cixi Tiandong Scale Factory Ultrapure water machine WP-UP-WF-40 Sichuan Water Treatment Equipment Co., Ltd. Digital constant temperature magnetic stirrer 85-2 Hangzhou Instrument Motor Co., Ltd. Dry heat aging box Bluepard BHO-401A Shanghai Yiheng Scientific Instrument Co., Ltd. Constant temperature blast drying oven DHG-9140B(101-2B) Shanghai Langgan Experimental Equipment Co., Ltd. Wet heat aging box HCP Meimerte (Shanghai) Trading Co., Ltd. Freeze-thaw aging chamber PT-2091BI Dongguan Baoda Instrument Co., Ltd. Tungsten Filament Scanning Electron Microscope SU3500 Hitachi High-Technologies Corporation Ion sputtering instrument BAL-TAC Swiss BAL-TEC Video Optical Contact Angle Tester KRUSS-DSA100 Germany KRUSS Company

[0062] Example 1

[0063] The breathable coating material provided in this embodiment includes the following raw materials in parts by weight: 10 parts of trifluorochloroethylene aqueous fluorine, 2.5 parts of sodium aluminosilicate, 2.5 parts of straw, 1.5 ml of dispersant and 85 parts of water.

[0064] In this embodiment, the straw is corn straw and the dispersant is octylphenol polyoxyethylene ether.

[0065] In this embodiment, the method for preparing the breathable coating material comprises the following steps:

[0066] S1. Take trifluorochloroethylene aqueous fluorine, sodium aluminosilicate, straw, dispersant and water according to the mass parts.

[0067] In this embodiment, each portion is weighed according to 1g, that is, 10g of trifluorochloroethylene aqueous fluoride, 2.5g of sodium aluminosilicate, 2.5g of straw, 1.5ml of dispersant and 85g of water are taken.

[0068] S2, washing and drying the straw, crushing and sieving after drying to obtain straw powder;

[0069] In this embodiment, the corn stalks are washed three times, placed in an oven at 80° C. for constant temperature drying, crushed and passed through a 120-mesh sieve, and stored at room temperature for later use.

[0070] S3. Mix 10g of trifluorochloroethylene aqueous fluorine, 2.5g of sodium aluminosilicate, 85g of ultrapure water and 2.5g of straw powder, add 1.5ml of dispersant, stir at 800r / min for 2h at 35°C, and stir evenly to obtain a breathable coating material.

[0071] Comparative Example 1

[0072] The coating material provided in this comparative example comprises the following raw materials in parts by mass: 10 parts of trifluorochloroethylene aqueous fluorine and 90 parts of water.

[0073] In this comparative example, the preparation method of the coating material comprises the following steps:

[0074] S1. Take trifluorochloroethylene aqueous fluorine and water according to the mass parts. Weigh 1g of each part, then take 10g of trifluorochloroethylene aqueous fluorine and 90g of water.

[0075] S2. Mix 10 g of trifluorochloroethylene aqueous fluorine and 90 g of ultrapure water, stir at 800 r / min for 2 h at a temperature of 35° C., and stir evenly to obtain a coating material.

[0076] Comparative Example 2

[0077] The coating material provided in this comparative example comprises the following raw materials in parts by mass: 10 parts of trifluorochloroethylene aqueous fluorine, 2.5 parts of sodium aluminosilicate, 2.5 parts of straw and 85 parts of water.

[0078] In this comparative example, the straw is corn straw.

[0079] In this comparative example, the preparation method of the coating material comprises the following steps:

[0080] S1. Take trifluorochloroethylene aqueous fluorine, sodium aluminosilicate, straw and water according to the mass parts. Weigh 1g of each part, then take 10g of trifluorochloroethylene aqueous fluorine, 2.5g of sodium aluminosilicate, 2.5g of straw and 85g of water.

[0081] S2, washing and drying the straw, crushing and sieving after drying to obtain straw powder;

[0082] In this embodiment, the corn stalks are washed three times, placed in an oven at 80° C. for constant temperature drying, crushed and passed through a 120-mesh sieve, and stored at room temperature for later use.

[0083] S3. Mix 10 g of trifluorochloroethylene aqueous fluorine, 2.5 g of sodium aluminosilicate, 85 g of ultrapure water and 2.5 g of straw powder, stir at 800 r / min for 2 h at 35° C., and stir evenly to obtain a coating material.

[0084] In order to verify the performance advantages of the breathable coating material of the present invention, the breathable coating materials provided in the embodiments and comparative examples were used to conduct the following tests.

[0085] Test 1: Physical properties test of films with different reinforcement coating materials

[0086] Test samples: the coating material of comparative example 1, the coating material of comparative example 2 and the breathable coating material provided in Example 1 are respectively denoted as coating 1, coating 2 and coating 3.

[0087] The test process is: take 5 ml of coating 1, coating 2 and coating 3 respectively and drop them into a 50mm*50mm*2mm silicone mold. After standing at a constant temperature of 25℃ for 48 hours, use tweezers to demold the mold to obtain three different reinforced coating material films.

[0088] (1) Take on-site photos of three different reinforcement coating material films, such as Figure 1 As shown, from left to right are coating 1, coating 2 and coating 3; and the morphology of the film is observed, and the results are shown in Table 2.

[0089] (2) Water absorption test: The three different reinforced coating material films obtained above were immersed in deionized water for 24 hours, and the weight of the films before and after water absorption was weighed to calculate the water absorption rate of the water-based fluorine film. Each group was measured three times and the average value was taken. The results are shown in Table 2.

[0090] (3) Surface hardness test: According to GB / T 6739-1996 "Paint film hardness pencil test method", the three different reinforced coating material films obtained above were tested for hardness. A pencil was held and pushed at a speed of 1 cm / s and 45 degrees for 1 cm, and the pushing was repeated five times. In the experiment, a pencil was found that scratched the film two or more times, and the hardness number after the hardness number of this pencil was recorded, which was the hardness value of the film. The results are shown in Table 2.

[0091] Table 2 Physical properties of three coating films

[0092]

[0093] See Table 2 and Figure 1 , a comprehensive comparison of the film performance from three aspects: water absorption, surface hardness and morphology. It can be seen that the film of coating 1 is uniform and has good surface hardness, but there are problems of wrinkling and cracking. The film of coating 2 is seriously warped and detached, which cannot fully protect the cultural relics of the earthen site from being damaged by external factors during long-term preservation; the film of coating 3 is uniform and has no bubbles, and the water absorption rate is 16.9%, which is slightly higher than that of other films; indicating that its surface hydrophobicity is reduced and its water permeability is improved. In addition, the surface hardness of coating 3 is good and has a certain toughness, and it is not easy to cause problems such as warping and cracking under stress.

[0094] Through comprehensive comparison, the breathable coating material (coating 3) of Example 1 has good film-forming effect and is most suitable for use as an anti-weathering coating in the protection of earthen ruins cultural relics. It can fully cover the surface of the cultural relics and achieve the expected protection effect.

[0095] Experiment 2: Fourier infrared analysis test of thin films with different reinforcement coating materials

[0096] Test samples: three different reinforced coating material films obtained from coating 1, coating 2 and coating 3 in test 1.

[0097] Experimental method: Fourier transform infrared spectrometer was used to test and analyze three different reinforcement coating material films at 4000 -1 ~400cm -1 The infrared spectrum test was analyzed within the range, and the results were as follows Figure 2 shown.

[0098] See also Figure 2 Infrared spectrum, 1727cm -1 The peak at 1074 cm is the C=O absorption peak. -1 and 1220cm -1 The stretching vibration absorption peaks of COC bond and CF bond are 935cm -1 It is the absorption peak of -OH bond in carboxylic acid. Comparing the infrared spectra of the three coatings, it is found that the absorption peak of -OH bond in coating 3 is sharper. However, the increase of hydroxyl group content helps to improve the hydrophilicity of the coating. Further, improving the hydrophilicity of the coating can enhance the wettability and penetration of the coating to solid cultural relics, thereby achieving better reinforcement and protection effect. At the same time, for coating 3, it is found that the characteristic groups of water-based fluorine of trifluorochloroethylene are still retained, indicating that coating 3 is still hydrophobic. It can be seen that the breathable coating material provided by the present invention is waterproof but not water-repellent, and meets the requirements for the protection of earthen ruins cultural relics.

[0099] Experiment 3. Microscopic morphology test of films made of different reinforcement coating materials. Test samples: three different reinforcement coating material films obtained from coating 1, coating 2 and coating 3 in Experiment 1.

[0100] Test method: The coating material film is fixed on the cross-section test bench with conductive glue, and the surface is treated with gold spraying for 120s with an ion sputtering instrument. The microscopic morphology of the film is observed under a tungsten filament scanning electron microscope at 500 times and 1000 times magnification, and the microstructure of the film cross section is studied and analyzed. The microscopic morphology of the cross section of the three different coating material films under tungsten filament scanning electron microscope at 50μm and 25μm is as follows: Figure 3 , Figure 4 and Figure 5 shown.

[0101] See also Figure 3 , Figure 4 and Figure 5 It can be seen that the cross-sectional structure of the trifluorochloroethylene water-based fluorine film is dense and has stratification. This is because the fluorine atom itself has extremely low surface energy, and the carbon fluorine chain segment is easy to migrate to the surface of the film. Although the trifluorochloroethylene water-based fluorine can protect the cultural relics from external damage to a certain extent as a coating, it also blocks the channels for the cultural relics of the earthen site to exchange gases and substances with the environment. In the long run, the cultural relics are prone to warping due to the failure of salt precipitation in time, destroying the original historical appearance of the cultural relics; and when only the modified coating with straw is added, its cross-section produces pores of different sizes and even partial voids due to the uneven distribution of corn straw, which is consistent with the phenomenon that the film of the above-mentioned coating 2 is severely warped and partially falls off; coating 3 is based on coating 2 and a dispersant is added to evenly disperse the straw powder in the coating, and finally a breathable film with equal pore size and uniform distribution is formed.

[0102] To sum up, at the microscopic level, the breathable coating material (coating 3) of Example 1 can improve the air permeability while ensuring that the structure of the coating itself is not excessively damaged, thereby effectively preventing the reduction of mechanical properties; at the macroscopic level, when used in the protection of earthen site cultural relics, it can play a good protective effect without hindering the exchange of substances and gases between the cultural relics and the outside world.

[0103] Test 4: Air permeability test

[0104] Test samples: the coating material of comparative example 1, the coating material of comparative example 2 and the breathable coating material provided in Example 1 are respectively denoted as coating 1, coating 2 and coating 3.

[0105] The test process is as follows:

[0106] (1) Sample preparation: Sandstone was collected from northern Shaanxi and cut into three 5*5*5 cm cubes. The dirt on the sample surface was removed using an ultrasonic cleaner and then dried in an oven at 105°C for 24 h to obtain three sandstone samples. Coating 1, coating 2, and coating 3 were evenly applied to the surfaces of the three sandstone samples using a soft-bristled brush. After drying at room temperature for 4 h, the coating was repeated three times to ensure that the sample surface was completely covered. Three simulated samples treated with different coatings were obtained.

[0107] (2) Test analysis: Take a 150 ml clean conical flask, fill it with an appropriate amount of deionized water, and place the three simulated samples on the flask respectively. Seal the joints with hydrophobic sludge to ensure that all water can only escape from the surface of the simulated sample. The whole device is weighed and recorded as the initial mass m0. Place it under constant temperature and humidity conditions (40°C open oven) for experimental testing. Each cycle is 72 hours. The mass of the whole device after weighing and testing is recorded as m1, that is, the water loss is m=m1-m0, and the air permeability coefficient is calculated. (t is the test time), accumulative test for 5 cycles, calculate the average air permeability coefficient (n is the test cycle), and the corresponding average air permeability coefficients of different simulated samples are obtained. The results are as follows Figure 6 shown.

[0108] from Figure 6 It can be seen that under constant temperature and humidity conditions, within the allowable error range, the air permeability of coating 3 and coating 2 is much better than that of coating 1. The average air permeability coefficient of coating 3 is 0.00586g / (25cm 2 h), the air permeability of coating 3 is 35.96% higher than that of coating 1. This is because the addition of straw powder destroys the original dense structure of water-based fluorine, making it loose and creating pores, thereby greatly improving the air permeability of the coating; in addition, the straw powder itself contains lignin, which is a complex aromatic polymer with a three-dimensional network structure. After high-temperature treatment, part of the lignin is thermally cracked, and small molecular gases are discharged, leaving pores, further improving the air permeability of the coating. Although the air permeability of coating 2 is also improved, adding only straw powder will result in uneven particle dispersion, affecting the leveling and film-forming properties of the coating, and reducing the adhesion between the coating and the earthen cultural relics.

[0109] It can be seen that the air permeability of the breathable coating material (coating 3) of Example 1 of the present invention is greatly improved, and it also has good leveling and film-forming properties, thereby improving the adhesion between the coating and the earthen cultural relics.

[0110] Test 5: Contact angle test

[0111] The size of the contact angle can reflect the difference in hydrophilicity and hydrophobicity of the material. The smaller the contact angle, the more hydrophilic the sample is, but too strong hydrophilicity will cause cultural relics to be easily damaged in a humid environment; the larger the contact angle, the more hydrophobic the sample is, which can prevent external pollutants from affecting cultural relics, but too strong hydrophobicity will significantly reduce the air permeability and water permeability of cultural relics, affecting their ability to exchange substances with the outside world. Therefore, appropriate hydrophilicity is one of the important criteria for screening whether the coating is suitable for application in cultural relic protection.

[0112] Test samples: the coating material of comparative example 1, the coating material of comparative example 2 and the breathable coating material provided in Example 1 are respectively denoted as coating 1, coating 2 and coating 3.

[0113] The test process is as follows: four sandstone samples of the same size are obtained by the method of test 4; then, coating 1, coating 2 and coating 3 are evenly applied on the surfaces of three of the sandstone samples, and the treatment after coating refers to test 4; the remaining sandstone sample is coated with any coating.

[0114] The three simulated samples and the untreated sandstone sample were placed on the optical contact angle test bench for contact angle test. Five points were taken for each group of samples for measurement, and the median was taken to compare the affinity of different groups of materials to water. The results are as follows: Figure 7 As shown, among them: (a) untreated sample, (b) sample treated with coating 1, (c) sample treated with coating 2, and (d) sample treated with coating 3.

[0115] See also Figure 7 It can be observed that: the contact angle of the unreinforced samples is extremely small, the hydrophilicity is very strong, and they are not resistant to external moisture intrusion; the samples treated with coating 1 have an average contact angle of 93.9°, which is very hydrophobic; the contact angles of the samples treated with coating 2 and coating 3 are slightly lower than those of coating 1, because the addition of corn straw powder and sodium aluminosilicate powder destroys the tight structure of trifluorochloroethylene water-based fluorine and increases its water permeability; the octylphenol polyoxyethylene ether in coating 3 not only acts as a dispersant to disperse, but also as a surfactant to reduce the surface tension of the film, improve its hydrophilicity, and increase the air permeability and water permeability of the cultural relics, which is consistent with the above permeability data.

[0116] Based on the above experiments, it can be seen that the breathable coating material (coating 3) of Example 1 of the present invention can ensure that the cultural relics have a certain degree of waterproofness, while not affecting the material and energy exchange capacity of the cultural relics themselves, and has a good protective effect on the earthen site cultural relics.

[0117] Test 6: Aging resistance test

[0118] This test tests the aging resistance from three aspects: dry heat aging, wet heat aging and freeze-thaw aging.

[0119] Test samples: the coating material of comparative example 1, the coating material of comparative example 2 and the breathable coating material provided in Example 1 are respectively denoted as coating 1, coating 2 and coating 3.

[0120] The test process is as follows: four sandstone samples of the same size are obtained by the method of test 4; then, coating 1, coating 2 and coating 3 are evenly applied on the surfaces of three of the sandstone samples, and the treatment after coating refers to test 4; the remaining one is a sandstone sample coated with any coating.

[0121] The test methods and conditions are as follows:

[0122] (1) Dry heat aging: The temperature of the dry heat aging chamber is 105℃±5℃

[0123] (2) Hygrothermal aging: The temperature of the hygrothermal aging chamber is 85°C ± 5°C, and the relative humidity is 65%.

[0124] (3) Freeze-thaw aging: The maximum temperature of the high and low temperature cycle aging box is 40℃±5℃, the minimum temperature is -30℃±5℃, the humidity is 50%, and one high and low temperature cycle is 8 hours.

[0125] With 7 days as a cycle, a total of 4 cycles were tested. The color difference between the simulated samples after each aging cycle and the corresponding samples before aging was tested. The color difference changes of the samples treated with three different coatings and the untreated samples after dry heat aging, wet heat aging, and freeze-thaw aging tests are shown as follows: Figure 8 , Fig. 9 and Fig.10 As shown; the aging resistance of different reinforced coating material samples was evaluated according to the color difference evaluation standard (see Table 3).

[0126] Table 3 Color difference evaluation standard

[0127] Color difference level Level Requirements ΔE value 0 No discoloration ≤1.50 1 Very slight discoloration 1.60~3.00 2 Slight discoloration 3.10~6.00 3 Obvious discoloration 6.10~9.00 4 Larger discoloration 9.10~12.00 5 Severe discoloration >12.00

[0128] See also Figure 8 , Fig. 9 and Fig.10In the dry heat aging and freeze-thaw aging tests, the unreinforced samples and the samples treated with coating 2 reached a slight discoloration level, while the samples treated with coating 1 and coating 3 showed very slight discoloration, indicating that coating 3 has a better protective effect than coating 1. This is because the straw powder contains lignin, which has certain antioxidant properties. Wet heat aging has the greatest impact on the samples. The simulated samples treated with the three coatings all achieved slight discoloration, but the color difference of the samples treated with coating 3 was the smallest. This is because coating 3 has good air permeability and can quickly discharge water vapor. The untreated sandstone samples have reached a significant discoloration level, which seriously damaged the original appearance of the samples. Among the three aging tests, coating 2 has the largest standard deviation because coating 2 is unevenly dispersed, which affects the leveling of the coating and prevents it from evenly protecting the entire sample surface.

[0129] Based on the results of the three aging tests, the breathable coating material (coating 3) of Example 1 of the present invention has the best anti-aging performance and can protect the cultural relics from discoloration for a long time without changing the original historical appearance after treatment.

[0130] The above-mentioned performance test of the coating material was carried out on a breathable coating material formed by 10 parts of trifluorochloroethylene aqueous fluorine, 2.5 parts of sodium aluminosilicate, 2.5 parts of straw, 1.5 ml of dispersant (octylphenol polyoxyethylene ether) and 85 parts of water. When other types of dispersants are selected or the mass ratio of the raw materials is changed, the breathable coating material obtained also shows an effect similar to that of the coating material in Example 1, that is, the coating material is waterproof but not water-repellent. While having good weather resistance and mechanical properties, it slightly reduces the hydrophobicity of the material, greatly improves the air permeability of the reinforced coating, and will not block the pores, so as to facilitate the exchange of matter and gas inside and outside the site, and has a good protective effect on the earthen site.

[0131] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A breathable coating material, It is characterized in that The invention comprises trifluorochloroethylene aqueous fluorine, aluminosilicate, straw, dispersant and water, wherein the mass ratio of trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and water is 5-15:1-5:1-5:75-95, and the volume of dispersant corresponding to every 10g of trifluorochloroethylene aqueous fluorine is 1ml-2ml.

2. The breathable coating material according to claim 1, It is characterized in that The mass ratio of trifluorochloroethylene aqueous fluorine, aluminosilicate, straw and water is 10:2.5:2.5:85, and the volume of the dispersant corresponding to every 10g of trifluorochloroethylene aqueous fluorine is 1.5ml.

3. The breathable coating material according to claim 1, It is characterized in that The straw is corn straw, rice straw or wheat straw; the dispersant is Tween-80, octylphenol polyoxyethylene ether, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate; the aluminosilicate is sodium aluminosilicate, potassium aluminosilicate or calcium aluminosilicate.

4. The breathable coating material according to claim 2, It is characterized in that The average air permeability coefficient of the breathable coating material is 0.00586 g / (25 cm 2 h).

5. The breathable coating material according to claim 2, It is characterized in that The air-permeable coating material has a water absorption rate of 16.9% and a contact angle of 75.5°.

6. A method for preparing the breathable coating material according to claim 1, It is characterized in that The preparation method comprises the following steps: S1. Take trifluorochloroethylene aqueous fluorine, aluminosilicate, straw, dispersant and water according to the mass parts; S2, washing and drying the straw, crushing and sieving after drying to obtain straw powder; S3, mixing aqueous fluorine of chlorotrifluoroethylene, aluminosilicate, water and the straw powder of step S2, adding a dispersant, stirring evenly, and obtaining a breathable coating material.

7. The preparation method according to claim 6, It is characterized in that In the step S2, the drying temperature is 75° C. to 85° C., the drying time is 24 h to 48 h, and the particle size of the straw powder is 80 mesh to 120 mesh.

8. The preparation method according to claim 6, It is characterized in that In step S3, the stirring conditions are: temperature 30°C to 40°C, stirring speed 600r / min to 1000r / min, and stirring time 1.5h to 2.5h.

9. Use of the breathable coating material as claimed in claim 1 in the protection of earthen ruins.

10. The use according to claim 9, It is characterized in that The application is to apply the breathable coating material as a coating on the inner wall of the earthen ruins.

Citation Information

Patent Citations

  • Earthen ruins return repair protecting agent

    CN103555086A

  • Method for preparing organic nano composite coating for stone historic preservation

    CN106497289A

  • Earth ruin composite reinforcement material and reinforcement process

    CN108395167A

  • Organic fluorosilicone-OvPOSS composite modified acrylate soap-free emulsion for earthen archaeological site protection

    CN116622035A