Rapid curing epoxy system conductive black ink suitable for copper foil substrate

By using a fast curing epoxy system composed of high molecular weight and medium molecular weight bisphenol A type epoxy resin on the surface of the copper foil, the problems of poor conductivity and high cost of conductive ink are solved, and efficient dispersion and rapid curing of ink are achieved. Improves conductivity and chemical resistance, suitable for high-precision applications.

CN118909488APending Publication Date: 2024-11-08SUZHOU BETELY POLYMER MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411181735.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing conductive inks have poor conductivity after coating the copper foil surface, are expensive, have a long curing time and unstable viscosity, which affects the quality and application range of copper foil coating materials.

Method used

A fast curing epoxy system consisting of high molecular weight and medium molecular weight bisphenol A solid epoxy resin, conductive carbon black, superconducting carbon black, amino resin, catalyst and coupling agent is formed by premixing and dispersing technology. Inks are grinded with a nano-sand mill to a fineness of ≤1μm to achieve efficient dispersion and rapid curing of ink.

Benefits of technology

It achieves rapid curing of ink, excellent conductivity, good chemical resistance and stable viscosity, and is suitable for high-precision application fields, reducing costs and expanding application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012372980000021
    Figure BDA0005012372980000021
  • Figure BDA0005012372980000031
    Figure BDA0005012372980000031
  • Figure BDA0005012372980000071
    Figure BDA0005012372980000071
Patent Text Reader

Abstract

The invention relates to rapid curing epoxy system conductive black ink suitable for a copper foil base material. The rapid curing epoxy system conductive black ink is prepared from high-molecular-weight bisphenol A type solid epoxy resin, bisphenol A type medium-molecular-weight solid epoxy resin, a solvent, a dispersing agent, conductive carbon black, superconductive carbon black, an auxiliary agent, amino resin, a catalyst and a coupling agent. The component A consists of bisphenol A type solid epoxy resin with high molecular weight, bisphenol A type medium molecular weight solid epoxy resin, a solvent, a dispersing agent, conductive carbon black, superconductive carbon black, an auxiliary agent, a catalyst and the like; the component B is composed of amino resin and a coupling agent; before use, the component A and the component B are premixed and dispersed for 15 minutes according to the weight ratio of 90: 10, are uniformly dispersed, and can be used after standing for half an hour.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to conductive ink, in particular to a conductive black ink suitable for a copper foil substrate and a fast-curing epoxy system. Background Art

[0002] Copper foil is a cathodic electrolytic material made of copper or copper alloy through rolling or electrolysis process. It is widely used in circuit boards, automotive electronics, satellite navigation, LED chips, and the new generation of 5G information network communication high-end industry. It is often used to manufacture conductive structures. It is an indispensable main raw material for the production of printed FCCL copper clad laminates, various fine circuit FPCs, LED substrates, and lithium-ion batteries or energy storage power supplies.

[0003] Generally, one side of high-precision copper foil is roughened to form a matte and rough interface to increase the peeling strength of metal materials, making it easy to laminate with other materials without falling off. However, the thickness tolerance of the copper foil treated by this process is unstable, the roughening surface has poor uniformity and flatness, which affects the conductivity of the copper foil, and has poor fatigue resistance, oxidation resistance, and mechanical properties.

[0004] Epoxy conductive black ink solves the above problems very well. A special laminated conductive material is formed by coating a layer of conductive ink on the surface of copper foil and curing it at high temperature. On the one hand, it improves the bonding strength between copper foil and substrate. On the other hand, the conductive ink coating can fill the tiny pits and holes on the rough single side of copper foil through self-leveling, forming a smooth, uniform, high-gloss black conductive coating on its surface, which greatly improves the conductivity, stability and precision of copper foil. Furthermore, the ink coating isolates oxygen and moisture, effectively preventing oxidation, blackening, corrosion and thermal expansion of copper foil, and also significantly contributes to improving bending resistance, elongation, fatigue resistance and mechanical properties. After curing, the epoxy conductive black ink forms a dense polymer structure, which makes the copper foil laminate material have excellent chemical resistance, alcohol resistance, ethyl ester resistance and toluene resistance, ensuring the reliable stability of the product, and also greatly expanding the application scenarios.

[0005] At present, the conductive black ink is coated on the surface of copper foil. Generally, the total film thickness of the ink is 2-3μm, and the resistance value or square resistance is 10^4Ω / Sq-10^6Ω / Sq. The main function is to provide antistatic effect, and the conductive performance is poor; another type of conductive ink is coated on the surface of copper foil, the ink thickness is 3-5μm, and the resistance value or square resistance of the copper foil laminated material is less than 50mΩ / Sq, such as a conductive ink suitable for double-light rolled copper foil disclosed in CN117701071A, which uses metal conductive particles such as conductive nickel powder, conductive silver powder, silver-coated copper powder, stone One or several graphenes are used as conductive media, which are extremely expensive and account for 40-60wt% in the formula, making the cost of conductive ink unacceptable to the market, which directly leads to the limitation of the actual application value of the invention, or a very small application range, and limited economic value. At the same time, the median particle size (D50) of the conductive particles is 2-5μm. After dispersion and grinding, the fineness of the finished ink product is between 3-5μm. After the ink coating is dried, its rough surface directly affects the conductivity, stability and precision of the copper foil cladding material.

[0006] Common gravure black inks suitable for coating the surface of copper foil substrates are prepared by mixing solvent-based saturated polyester or polyester polyol, polyurethane as the main connecting material, and carbon-based, metal conductive particles or mixtures as the conductive medium. Since the resin structure is mostly a straight-chain structure, the resin itself is relatively soft and has a low cross-linking density. The main disadvantage is poor alcohol resistance, and poor resistance to ester and aromatic hydrocarbon solvents. Another type is an ink prepared by using one or more of the solvent-based acrylic polyol resins as the main connecting material. After the terminal hydroxyl groups of the acrylic polyol resin molecular chains are cross-linked with isocyanate curing agents, the solvent resistance of the ink is improved, but the disadvantages are long curing time, poor coating flexibility and poor adhesion. Moreover, these types of two-liquid or multi-liquid curing reaction systems will also undergo cross-linking reactions in the ink during construction at room temperature, and the viscosity and performance characteristics of the ink will change accordingly, which seriously affects the construction characteristics of the ink and the physical and chemical properties of the ink coating, and brings potential risks to the product quality of copper foil laminated materials.

[0007] Therefore, it is necessary to provide a fast-curing epoxy conductive black ink suitable for copper foil substrates to solve the above problems. Summary of the invention

[0008] The invention aims to provide a fast-curing epoxy conductive black ink suitable for a copper foil substrate.

[0009] The present invention achieves the above object through the following technical solutions:

[0010] Technical solution:

[0011] A fast-curing epoxy conductive black ink suitable for copper foil substrates, comprising high molecular weight bisphenol A type solid epoxy resin, bisphenol A type medium molecular weight solid epoxy resin, solvent, dispersant, conductive carbon black, superconducting carbon black, additive, amino resin, catalyst, and coupling agent;

[0012] Component A is composed of high molecular weight bisphenol A type solid epoxy resin, bisphenol A type medium molecular weight solid epoxy resin, solvent, dispersant, conductive carbon black, superconducting carbon black, additives, catalyst, etc.;

[0013] Amino resin and coupling agent constitute component B;

[0014] Before use, premix component A and component B in a weight ratio of 90 / 10, disperse for 15 minutes, disperse evenly, and let stand for half an hour before use.

[0015] Furthermore, in percentage terms:

[0016] Component A:

[0017]

[0018]

[0019] Component B:

[0020] 6-10 parts of amino resin;

[0021] 1-2 parts of coupling agent.

[0022] Furthermore, the high molecular weight bisphenol A type solid epoxy resin is one or more of the American DOW DOW solid epoxy resin DER669E, DER669-20, Nanya NPES-909, NPES-909H, with an epoxy equivalent (g / eq.) of 1800-5500, wherein the epoxy equivalent (g / eq.) is preferably 3500; it is solid granular at room temperature and has a solid content of 100%; the resin Tg point is generally between 120°C and 165°C; combined with the medium molecular weight bisphenol A type solid epoxy resin, after reacting with the amino resin, a dense and tough film layer is formed, which has excellent alcohol and solvent resistance.

[0023] Furthermore, the bisphenol A medium molecular weight solid epoxy resin is one or more of the American DOW solid epoxy resin DER664UE, DER 663UE, Nanya's NPES-903H, NPES-904, NPES-905L, with an epoxy equivalent (g / eq.) of 740-930, wherein the epoxy equivalent (g / eq.) is preferably 900; it is solid granular at room temperature and has a solid content of 100%; the resin Tg point is generally between 90°C and 110°C; the bisphenol A medium molecular weight solid epoxy resin is used as the main film-forming binder of the ink, has extremely strong adhesion to substrates such as metal and glass, and at the same time provides excellent flexibility, interlayer adhesion, chemical resistance, corrosion resistance, and temperature resistance after the ink is formed into a film.

[0024] Furthermore, the dispersant is one or more of AFCONA-7525, EFKA-5210, and Lubrizol's SOLSPERSE(TM) 20000C super dispersant, which is used to wet and disperse pigments, has good viscosity characteristics, and suppresses the performance of highly filled systems; with the grinding process, the carbon black particles can be extremely evenly dispersed in the resin system with a sub-nanometer particle size to form a uniform and stable black slurry, and the carbon black particles are not prone to re-aggregation in the resin system, and the ink is not prone to adverse phenomena such as coarsening, floating color, and solvent precipitation; in addition, the viscosity-reducing effect of the dispersant increases the fluidity of the ink, and also has a positive effect on the leveling and film-forming surface effects of the ink; high solid and low viscosity, to achieve excellent color development and excellent hiding power of the ink.

[0025] Furthermore, the conductive carbon black is one or more of the super-dense high-conductive carbon black SUPER P Li, CABOT superconducting carbon black VULCANXC-72R, Aksu Kechen Black EC300J, and Aksu Kechen Black ECP-600JD, which have high structure, high blackness, good hiding power, and strong conductivity. When combined with a suitable dispersant, it can provide the ink with excellent conductive properties and hiding effects. In addition, a suitable dispersant is combined with carbon black and ground by a nano sand mill to form a sub-nanoscale conductive black ink, in which the gap between the conductive media is extremely small, further improving the conductive properties of the ink coating.

[0026] Furthermore, the solvent is one or more of butanone, cyclohexanone, PMA, BCS, PM, and methyl isobutyl ketone. The solvents are used in combination to optimize the solubility of the solvent relative to the solubility of the resin. Combined with the resin formula and the dispersant, the ink stability can be improved and the ink storage time can be extended. The appropriate solvent evaporation rate has a higher efficiency in the solvent evaporation stage during the rapid curing process of the ink, and plays an extremely important role in the surface drying effect of the ink. Among them, butanone, PM, methyl isobutyl ketone, and cyclohexanone are preferred.

[0027] Furthermore, the additive is one or more of BYK-3560, BYK-354, and Huaxia additive HX-3060, and the additive is a silicone leveling agent or a silicone-free leveling agent, which promotes the surface leveling effect of the ink layer after coating; at the same time, it promotes the wettability of the ink system to the substrate, thereby increasing the adhesion of the ink to the surface of the substrate.

[0028] Furthermore, the amino resin is CYMEL 325 amino resin, CYMEL 701 amino resin, MR-625S amino resin from Changchun Chemical, RESIMENE One or more of the 717 amino resins are partially methylated amino resins, which only require weak acid catalysis, low temperature reaction, quick drying, high hardness, high gloss, and excellent chemical resistance; the low acid value of the main resin matched with it is sufficient to catalyze the crosslinking reaction, and organic or inorganic weak acid catalysis such as maleic acid, citric acid, phosphoric acid, alkyl phosphoric acid, a small amount of p-toluenesulfonic acid and other catalysts can also be added to achieve low-temperature rapid curing; in a weak alkaline system or a system with an appropriate amount of n-butanol and no catalyst, the reaction rate is extremely slow at room temperature <35°C, and the storage time is as long as 6 months, which provides favorable conditions for the construction of ink at room temperature, that is, the ink system prepared by it does not react or has an extremely slow reaction rate below 35°C at room temperature, and the viscosity, state, and performance of the ink are relatively stable for a long time. After coating by gravure printing process, the curing reaction can be completed at 160±5°C / 3Min, and the ink coating exhibits excellent physical and chemical properties, such as hardness and chemical resistance.

[0029] Furthermore, the coupling agent is one or more of the siloxane coupling agents KH570, KH-792, Dow Corning Z-6011, Z-6020, and Z-6030, and the coupling agent is methacrylate silane or amino or bisamino silane, which can be used to improve the adhesion of organic resins to inorganic surfaces, improve the adhesion of resins to inorganic substrates such as metals and glass, and can significantly improve the wet abrasion resistance, wear resistance, and high temperature resistance of the coating.

[0030] Furthermore, the catalyst is American Jin One or more of 2500 p-toluenesulfonic acid catalyst and King's NACURE-5076 acid catalyst are used to accelerate the curing of some etherified amino resins at normal baking temperature, reduce the reaction temperature, shorten the reaction time, and achieve rapid curing.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1) After coating by gravure printing process, the curing reaction can be completed at 160±5℃ / 3Min, and the obtained ink coating exhibits excellent physical and chemical properties, such as hardness, chemical resistance, moisture resistance, etc.; at the same time, it does not react or has an extremely slow reaction rate at room temperature below 35℃, which ensures that the viscosity, state and performance of the ink are relatively stable for a long time, a long activation period of more than 48H, and good construction properties, which further ensure the quality of the ink coating and the reliability of its performance.

[0033] 2) The coated copper foil laminated material of the present invention has ultra-high gloss, smooth and uniform surface, excellent conductivity, and square resistance ≤50mΩ / Sq, which is particularly suitable for application fields with high requirements for conductive performance and precision. Specifically, a special laminated conductive material is formed by coating a layer of conductive ink on the surface of the copper foil and curing it at high temperature. On the one hand, it can improve the bonding force between the copper foil and the substrate. On the other hand, the ultra-high gloss conductive ink with a gloss of 120±5Gs has excellent self-leveling properties. The coating can fill the tiny pits and holes on the rough single side of the copper foil through self-leveling, forming a smooth, flat and uniform high-gloss black conductive coating on its surface, which greatly improves the conductivity, stability and precision of the copper foil.

[0034] 3) The coated copper foil laminate material of the present invention has high gloss, strong ink hiding power, and an ink film thickness of less than 1 μm, without leakage of the copper bottom; the ultra-thin ink coating of less than 1 μm can isolate oxygen, moisture, etc., effectively prevent the copper foil from oxidation, blackening, corrosion and thermal expansion, and also significantly contribute to improving the bending resistance, elongation, fatigue resistance, mechanical properties, and electrical conductivity; the epoxy system conductive black ink forms a dense polymer structure after curing, so that the copper foil laminate material has excellent chemical resistance, alcohol resistance, ethyl ester resistance, toluene resistance, etc., which ensures the reliable stability of the product and greatly expands the application scenarios.

[0035] 4) After the curing of the present invention is completed, the alcohol resistance is 500g / f, >1000 times, the ethyl ester resistance is 500g / f, >1000 times, and the toluene resistance is 500g / f, >1000 times, with excellent performance.

[0036] 5) The present invention does not react or has an extremely slow reaction rate below room temperature of 35°C, which ensures that the viscosity, state and performance of the ink are relatively stable for a long time, has a long activation period of more than 48 hours, and has good construction properties, which further ensures the quality and performance reliability of the ink coating; it solves the problems of short activation period and poor construction stability of common products. For example, the reaction system using hydroxyl acrylic resin, polyester, polyurethane resin, etc. as a connecting material and isocyanate curing agent as a cross-linking agent has a short product activation period, a fast increase in ink viscosity during construction, and poor performance stability, which directly affects the quality reliability of copper foil laminated material products.

[0037] 6) The epoxy resin involved in the present invention is dissolved in a specific proportion by solvents of different gradients and solubilities to form a stable transparent solution. The resin solution is used as a base material, supplemented with specific carbon-based conductive materials, dispersants, additives, catalysts, etc., and ground to a fineness of ≤1μm to form a stable black ink system A component, and conductive media such as superconducting carbon black form a more compact conductive network in the ink, which has a smaller square resistance, better conductivity, and is not easy to agglomerate; specifically, the copper foil laminated material prepared by the conductive black ink provided by the present invention has high gloss, a smooth and uniform surface, and excellent conductivity. In particular, when the ink coating thickness is less than 1 micron, the copper foil laminated material has a square resistance of ≤50mΩ / Sq, which is particularly suitable for application fields with high requirements for conductive performance and precision.

[0038] 7) The copper foil laminated material is coated with a fast-curing epoxy conductive black ink suitable for a copper foil substrate as described in the present invention. On the one hand, the bonding strength between the copper foil and the substrate is improved. On the other hand, the conductive ink coating can well fill the tiny pits and holes on the rough single side of the copper foil through self-leveling, forming a smooth, flat and uniform high-gloss black conductive coating on its surface, which greatly improves the conductivity, stability and precision of the copper foil laminated material. Furthermore, the ink coating plays a role in isolating oxygen and moisture, etc., effectively preventing the copper foil from oxidation, blackening, corrosion and thermal expansion, and also has a significant contribution to improving the bending resistance, elongation, fatigue resistance, mechanical properties, etc.

[0039] 8) After curing, the surface tension of the present invention is ≥50Dyn, and the peeling force is ≥2050g / f. The higher surface tension is conducive to lamination with other materials or adhesives. DETAILED DESCRIPTION

[0040] Example:

[0041] A fast-curing epoxy conductive black ink suitable for copper foil substrates, comprising high molecular weight bisphenol A type solid epoxy resin, bisphenol A type medium molecular weight solid epoxy resin, solvent, dispersant, conductive carbon black, superconducting carbon black, additive, amino resin, catalyst, coupling agent, etc. The high molecular weight bisphenol A type solid epoxy resin, bisphenol A type medium molecular weight solid epoxy resin, solvent, dispersant, conductive carbon black, superconducting carbon black, additive, and catalyst constitute component A; amino resin and coupling agent constitute component B; before use, premix component A and component B at a weight ratio of 90 / 10, disperse for 15 minutes, and let stand for half an hour after even dispersion before use.

[0042] All raw materials involved in the present invention are commercially available products, and the specific preparation operations and testing methods are conventional technologies; the creativity of the present invention lies in the selection of formulas, the combination of components and the technical effects brought about; each weight portion is 1 kg; the stirring device in the production step is specifically a disperser. The grinder is specifically a nano sand grinder, and the grinding fineness is required to be ≤1 μm. The maximum particle size of the filter bag used is 0.5 microns.

[0043] Embodiment 1

[0044] 1. Add the dispersant to the solvent (3 or 4 solvents, 25 wt% each) according to the proportion and disperse at a speed of 600 r / min for 5 minutes, then add the conductive carbon black while stirring, and then disperse at a speed of 600 r / min for 15 minutes, and let it stand for 2 hours for use;

[0045] 2. After step 1, pour the resin and solvent (three or four solvents, 50 wt% each) into the reaction kettle according to the formula ratio, heat to 60°C while stirring, keep warm for 4 hours until completely dissolved, filter through 400 mesh, and set aside;

[0046] 3. Add the carbon slurry prepared in step 1 into step 2 and disperse it at a speed of 600 r / min for 15 minutes;

[0047] 4. Pour the dispersed material in step 3 into a sand mill for grinding to obtain a semi-finished product;

[0048] 5. Add the remaining solvent, additives and catalyst to the semi-finished product obtained in step 3, stir and disperse evenly, filter with a 0.5 micron filter bag to obtain component A suitable for the finished product of the fast-curing epoxy conductive black ink on the copper foil substrate.

[0049] 6. Disperse the coupling agent into the amino resin according to the proportion and disperse it at a speed of 300r / min for 15 minutes to obtain component B. Keep the working environment dry and the relative humidity of the air less than 50% rh.

[0050] Component A and component B make up the ink. They should be premixed in proportion for 15 minutes before coating. After being evenly dispersed, filter with a 0.5-micron filter bag and let stand for half an hour before use.

[0051] By weight, the formula is as follows:

[0052] Component A:

[0053]

[0054] Component B:

[0055] Amino resin CYMEL 701 8 parts;

[0056] 2 parts of coupling agent Z-6020.

[0057] Embodiment 2

[0058] 1. Add the dispersant to the solvent (3 or 4 solvents, 25 wt% each) according to the proportion and disperse at a speed of 600 r / min for 5 minutes, then add the conductive carbon black while stirring, and then disperse at a speed of 600 r / min for 15 minutes, and let it stand for 2 hours for use;

[0059] 2. After step 1, pour the resin and solvent (three or four solvents, 50 wt% each) into the reaction kettle according to the formula ratio, heat to 60°C while stirring, keep warm for 4 hours until completely dissolved, filter through 400 mesh, and set aside;

[0060] 3. Add the carbon slurry prepared in step 1 into step 2 and disperse it at a speed of 600 r / min for 15 minutes;

[0061] 4. Pour the dispersed material in step 3 into a sand mill for grinding to obtain a semi-finished product;

[0062] 5. Add the remaining solvent, additives and catalyst to the semi-finished product obtained in step 3, stir and disperse evenly, filter with a 0.5 micron filter bag to obtain component A suitable for the finished product of the fast-curing epoxy conductive black ink on the copper foil substrate.

[0063] 6. Disperse the coupling agent into the amino resin according to the proportion and disperse it at a speed of 300r / min for 15 minutes to obtain component B. Keep the working environment dry and the relative humidity of the air less than 50% rh.

[0064] Component A and component B make up the ink. They should be premixed in proportion for 15 minutes before coating. After being evenly dispersed, filter with a 0.5-micron filter bag and let stand for half an hour before use.

[0065] By weight, the formula is as follows:

[0066] Component A:

[0067]

[0068] Component B:

[0069] Amino resin MR-625S 8 parts;

[0070] Coupling agent KH-792 2 parts.

[0071] Embodiment 3

[0072] 1. Add the dispersant to the solvent (3 or 4 solvents, 25 wt% each) according to the proportion and disperse at a speed of 600 r / min for 5 minutes, then add the conductive carbon black while stirring, and then disperse at a speed of 600 r / min for 15 minutes, and let it stand for 2 hours for use;

[0073] 2. After step 1, pour the resin and solvent (three or four solvents, 50 wt% each) into the reaction kettle according to the formula ratio, heat to 60°C while stirring, keep warm for 4 hours until completely dissolved, filter through 400 mesh, and set aside;

[0074] 3. Add the carbon slurry prepared in step 1 into step 2 and disperse it at a speed of 600 r / min for 15 minutes;

[0075] 4. Pour the dispersed material in step 3 into a sand mill for grinding to obtain a semi-finished product;

[0076] 5. Add the remaining solvent, additives and catalyst to the semi-finished product obtained in step 3, stir and disperse evenly, filter with a 0.5 micron filter bag to obtain component A suitable for the finished product of the fast-curing epoxy conductive black ink on the copper foil substrate.

[0077] 6. Disperse the coupling agent into the amino resin according to the proportion and disperse it at a speed of 300r / min for 15 minutes to obtain component B. Keep the working environment dry and the relative humidity of the air less than 50% rh.

[0078] Component A and component B make up the ink. They should be premixed in proportion for 15 minutes before coating. After being evenly dispersed, filter with a 0.5-micron filter bag and let stand for half an hour before use.

[0079] By weight, the formula is as follows:

[0080] Component A:

[0081]

[0082] Component B:

[0083] 8 parts of amino resin RESIMENE 717;

[0084] 2 parts of coupling agent Z-6020.

[0085] Performance Testing:

[0086] Taking Example 2 as an example, the above-mentioned component A, component B, and diluent (methyl ethyl ketone) of the conductive black ink suitable for rapid curing epoxy system on copper foil substrate are mixed evenly according to the mass ratio of 90:10:30, filtered with a 0.5 micron filter bag, and gravure coated on the machine. The coating method is the existing method without primer; the roller applies the ink to the substrate and bakes it in a hot air oven at 160±5℃ for 3 minutes, and it can be rolled up after cooling; after standing at room temperature for 2 hours, the curing is completed, and the relevant performance test can be carried out. The substrate is 10 micron electrolytic copper foil (supplier: Longdian Huaxin) and 10 micron rolled copper foil (supplier: Shanghai Jiaxian).

[0087] Table 1 takes Example 2 as an example, and after coating and curing, the ink performance is tested:

[0088]

[0089]

[0090] Table 2 compares the performance of the ink obtained in Example 2 with the competitive ink used by most domestic printing plants:

[0091]

[0092] The base material is 10-micron single-sided roughened copper foil material, and the suppliers are Longdian Huaxin and Shanghai Jiaxian.

[0093] The present invention uses one or more epoxy resins in a certain proportion, dissolves them in solvents with different gradients and solubilities in a specific proportion to form a stable transparent solution, uses the resin solution as a base material, and is supplemented with a specific carbon-based conductive material, a dispersant, an auxiliary agent, a catalyst, etc., and is ground to a fineness of ≤1 μm to form a component A of a stable black ink system, so that the ink forms a more compact conductive network, has a smaller square resistance, better conductivity, and is not easy to agglomerate or settle; and uses a component B with amino resin and a silane coupling agent as main components as a crosslinking agent, and completes a curing reaction by heating; the component A of the ink system does not react or has an extremely slow reaction rate (storage period of up to 6 months) at room temperature (below 35° C.), and has a long activation period (>48 hours, The ink has stable performance and very little viscosity change). After being coated on the surface of the substrate by gravure printing process, the curing reaction can be quickly completed by meeting the thermal curing condition of 160±5℃ / 3Min. The black ink coating formed after curing and cross-linking has high gloss (gloss 120±5Gs), strong ink hiding power (ink film thickness <1μm, no leakage of copper bottom), high blackness (L value <24), alcohol resistance (500g / f, >1000 times), ethyl acetate resistance (500g / f, >1000 times), toluene resistance (500g / f, >1000 times) and other excellent properties. What is important is that the copper foil cladding material prepared by the conductive black ink provided by the present invention has ultra-high gloss, smooth and uniform surface, excellent conductivity (square resistance ≤50mΩ / Sq), and is particularly suitable for application fields with high requirements for conductive performance and precision.

[0094] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A fast curing epoxy conductive black ink suitable for copper foil substrate, characterized in that: It is composed of high molecular weight bisphenol A type solid epoxy resin, bisphenol A type medium molecular weight solid epoxy resin, solvent, dispersant, conductive carbon black, superconducting carbon black, additive, amino resin, catalyst and coupling agent; Component A is composed of high molecular weight bisphenol A type solid epoxy resin, bisphenol A type medium molecular weight solid epoxy resin, solvent, dispersant, conductive carbon black, superconducting carbon black, additives, catalyst, etc.; Amino resin and coupling agent constitute component B; Before use, premix component A and component B at a weight ratio of 90 / 10, disperse for 15 minutes, disperse evenly, and let stand for half an hour before use; In percentage terms: Component A: Component B: 6-10 parts of amino resin; 1-2 parts of coupling agent.

2. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The high molecular weight bisphenol A type solid epoxy resin is one or more of the American DOW solid epoxy resin DER 669E, DER669-20, Nan Ya's NPES-909, NPES-909H, with an epoxy equivalent (g / eq.) of 1800-5500, wherein the epoxy equivalent (g / eq.) is preferably 3500; it is solid granular at room temperature, with a solid content of 100%; the resin Tg point is generally between 120°C and 165°C; combined with the medium molecular weight bisphenol A type solid epoxy resin, after reacting with the amino resin, a dense and tough film layer is formed, which has excellent alcohol resistance and solvent resistance.

3. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The bisphenol A type medium molecular weight solid epoxy resin is one or more of the American DOW DOW solid epoxy resin DER 664UE, DER 663UE, Nanya NPES-903H, NPES-904, NPES-905L, epoxy equivalent (g / eq.) 740-930, wherein the epoxy equivalent (g / eq.) 900 is preferred; it is solid granular at room temperature, with a solid content of 100%; the resin Tg point is generally between 90°C and 110°C; the bisphenol A type medium molecular weight solid epoxy resin is used as the main film-forming binder of the ink, has extremely strong adhesion to substrates such as metal and glass, and provides excellent flexibility, interlayer adhesion, chemical resistance, corrosion resistance, and temperature resistance of the ink after film formation.

4. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The dispersant is one or more of AFCONA-7525, EFKA-5210, and Lubrizol's SOLSPERSE(TM)20000C super dispersant, which is used to wet and disperse pigments, and has good viscosity characteristics and high-filling system suppression performance. With the grinding process, the carbon black particles can be dispersed in the resin system with a sub-nanometer particle size and extremely uniformly to form a uniform and stable black slurry. The carbon black particles are not easy to re-aggregate in the resin system, and the ink is not prone to adverse phenomena such as coarsening, floating color, and solvent precipitation. In addition, the viscosity-reducing effect of the dispersant increases the fluidity of the ink, and also has a positive effect on the leveling and film-forming surface effects of the ink. High solid and low viscosity achieve excellent color development and excellent hiding power of the ink.

5. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The conductive carbon black is one or more of the super-dense high-conductive carbon black SUPER P Li, CABOT superconductive carbon black VULCAN XC-72R, Aksu Kechen Black EC300J, and Aksu Kechen Black ECP-600JD, which has high structure, high blackness, good hiding power, and strong conductivity. With the appropriate dispersant selection, it can provide the ink with excellent conductive properties and hiding effects; in addition, a suitable dispersant is combined with carbon black, and ground by a nano sand mill to form a sub-nanometer conductive black ink, the gap between the conductive media is extremely small, which further improves the conductive properties of the ink coating.

6. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The solvent is one or more of butanone, cyclohexanone, PMA, BCS, PM, and methyl isobutyl ketone. The solvents are used in combination to optimize the solubility of the solvent relative to the solubility of the resin. Combined with the resin formula and the dispersant, the ink stability can be improved and the ink storage time can be extended. The appropriate solvent evaporation rate has a higher efficiency in the solvent evaporation stage during the rapid curing process of the ink, and plays an extremely important role in the surface drying effect of the ink. Among them, butanone, PM, methyl isobutyl ketone, and cyclohexanone are preferred.

7. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The additive is one or more of BYK-3560, BYK-354, and Huaxia additive HX-3060. The additive is a silicone leveling agent or a silicone-free leveling agent, which promotes the surface leveling effect of the ink layer after coating; at the same time, it promotes the wettability of the ink system to the substrate, thereby increasing the adhesion of the ink to the substrate surface.

8. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The amino resins are CYMEL 325 amino resin, CYMEL 701 amino resin, MR-625S amino resin from Changchun Chemical, and RESIMENE from INEOS. One or more of the 717 amino resins are partially methylated amino resins, which only require weak acid catalysis, low temperature reaction, quick drying, high hardness, high gloss, and excellent chemical resistance; the low acid value of the main resin matched with it is sufficient to catalyze the crosslinking reaction, and organic or inorganic weak acid catalysis such as maleic acid, citric acid, phosphoric acid, alkyl phosphoric acid, a small amount of p-toluenesulfonic acid and other catalysts can also be added to achieve low-temperature rapid curing; in a weak alkaline system or a system with an appropriate amount of n-butanol and no catalyst, the reaction rate is extremely slow at room temperature <35°C, and the storage time is as long as 6 months, which provides favorable conditions for the construction of ink at room temperature, that is, the ink system prepared by it does not react or has an extremely slow reaction rate below 35°C at room temperature, and the viscosity, state, and performance of the ink are relatively stable for a long time. After coating by gravure printing process, the curing reaction can be completed at 160±5°C / 3Min, and the ink coating exhibits excellent physical and chemical properties, such as hardness and chemical resistance.

9. The fast curing epoxy conductive black ink suitable for copper foil substrate according to claim 1, characterized in that: The coupling agent is one or more of the siloxane coupling agents KH570, KH-792, Dow Corning Z-6011, Z-6020, and Z-6030. The coupling agent is methacrylate silane or amino or bisamino silane, which can be used to improve the adhesion of organic resins to inorganic surfaces, improve the adhesion of resins to inorganic substrates such as metals and glass, and can significantly improve the wet abrasion resistance, wear resistance, and high temperature resistance of the coating.

10. A fast curing epoxy conductive black ink suitable for copper foil substrate according to any one of claims 1 to 9, characterized in that: The catalyst is American Jinshi One or more of 2500 p-toluenesulfonic acid catalyst and King's NACURE-5076 acid catalyst are used to accelerate the curing of some etherified amino resins at normal baking temperature, reduce the reaction temperature, shorten the reaction time, and achieve rapid curing.