Basic powder coating for vehicle body as well as preparation method and application of basic powder coating
By preparing and applying the basic powder coating, the automotive surface decoration process is simplified, and the problems of complex processes, VOC emissions and vehicle paint damage in the prior art are solved, thereby achieving more efficient, environmentally friendly and economical automotive surface protection.
Patent Information
- Application Number
- CN202411268044.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-08
AI Technical Summary
The existing automotive surface decoration protection process is complex, has low efficiency, high cost, and has problems with volatile organic compounds (VOC) emissions, as well as possible damage during vehicle paint replacement, which increases repair costs.
A basic powder coating and preparation method thereof are adopted, including resin, curing agent, benzoin, leveling agent, auxiliary degassing agent, pigment filler and powdering additive, and particles are formed by mixing, extruding, cooling, crushing, and grinding. The powder coating with a diameter of 28-45μm is electrostatically sprayed and baked and cured, and then applied to the car coat to simplify the process flow.
It effectively reduces VOC emissions, avoids damage to the car paint, reduces repair costs, and improves environmental protection and economic benefits.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of vehicle body treatment, and in particular to a basic powder coating for a vehicle body and a preparation method and application thereof. Background Art
[0002] The existing automobile surface decoration and protection mainly adopts paint coating technology, generally using electrophoresis + primer + base paint + clear varnish process.
[0003] For example, Chinese patent CN116239927B proposes a vehicle body coating structure with a ceramic effect and a preparation method thereof, wherein the coating structure comprises an electrophoretic layer, a first base paint layer, a second base paint layer, a pearlescent paint layer and a varnish layer stacked in sequence; the first base paint layer is formed by curing the first base paint; the two layers of base paint have the same color to reduce mutual covering between layers, and the base paint layer has a high overall covering power, and an engineering covering of 28-30μm film thickness can be achieved on the electrophoretic layer with an L value of 10-45, reducing pinholes and sagging in the paint film, giving the vehicle body a high-purity white ceramic effect.
[0004] However, the electrophoresis + primer + base coat + clear coat process adopted in the above patent is not only complicated in process and inefficient but also has a very serious VOC (volatile organic compound) emission problem during the painting process; in addition, the paint may be damaged when the car cover needs to be replaced later, which increases the additional repair cost.
[0005] Based on this, the present invention designs a basic powder coating for a vehicle body and a preparation method and application thereof to solve the above-mentioned problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a basic powder coating for a vehicle body and a preparation method and application thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: A basic powder coating for a car body, comprising the following raw materials in parts by weight: 55-80 parts of resin, 3-18.5 parts of curing agent, 0.2-2 parts of benzoin, 0.5-1.8 parts of leveling agent, 0-1.5 parts of auxiliary degassing agent, 10-30 parts of pigments and fillers, 0-0.5 parts of powdering agent; The resin is selected from one of saturated carboxylic acid polyester resin, saturated hydroxyl polyester resin or GMA type acrylic resin, and the curing agent is selected from one of TGIC curing agent, HAA curing agent, isocyanate curing agent or long-chain dicarboxylic acid.
[0008] Furthermore, the leveling agent is a polyacrylate compound loaded with gas silicon.
[0009] Furthermore, the auxiliary degassing agent is an amino-modified phenol urea surfactant.
[0010] Furthermore, the pigment filler consists of barium sulfate, titanium dioxide and carbon black.
[0011] Furthermore, the mass ratio of the barium sulfate, titanium dioxide and carbon black is (10-30):(0.5-5):(0-0.1).
[0012] A method for preparing the basic powder coating comprises the following steps: Step 1: weigh 55-80 parts of resin, 3-18.5 parts of curing agent, 0.2-2 parts of benzoin, 0.5-1.8 parts of leveling agent, 0-1.5 parts of auxiliary degassing agent, 10-30 parts of pigments and fillers, and 0-0.5 parts of powdering agent; The resin is selected from one of saturated carboxylic acid polyester resin, saturated hydroxyl polyester resin or GMA type acrylic resin, and the curing agent is selected from one of TGIC curing agent, HAA curing agent, isocyanate curing agent or long-chain dicarboxylic acid; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A, tableting, crushing, and grinding it into powder; Step 5: Sieve the powder to obtain a basic powder coating with a normally distributed particle size.
[0013] Furthermore, the leveling agent in step 1 is a polyacrylate compound loaded with gas silicon, and the auxiliary degassing agent is an amino-modified phenol urea surfactant.
[0014] Furthermore, in step five, the powder is passed through a 180-mesh sieve.
[0015] Furthermore, the average particle size of the basic powder coating in step 5 is 28-45 μm.
[0016] The invention discloses an application of a basic powder coating in automobile surface treatment, wherein a layer of the basic powder coating is electrostatically sprayed on a car body, and then baked and cured in a baking oven at 150-200° C. for 10-20 minutes, and a car cover is pasted on the outer side of the basic powder coating after curing.
[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention effectively reduces the emission of VOC (volatile organic compounds), thereby improving environmental benefits, while avoiding the damage to the car paint that may occur when the car cover needs to be replaced later, reducing the repair cost and having good economic benefits. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1
[0019] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 80kg saturated carboxylic acid polyester resin, 6.2kg TGIC curing agent, 2kg benzoin, 1.8kg leveling agent, 1.5kg auxiliary degassing agent, 30kg pigment filler, and 0.5kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment and filler are composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 30:5:0.1; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a base powder coating with an average particle size of 30-45 μm; Before the car leaves the factory, a layer of basic powder coating prepared by the above method is electrostatically sprayed. This coating has good adhesion to the car body substrate (≤1 level, GB / T 9286-1998) and good construction compatibility with the subsequent car cover, which is used for basic protection and primer. Then the car cover selected by the customer is attached to the outside of the coating, that is, the "basic powder coating + car cover" technical solution is adopted to complete the surface decoration and protection of the car body. When the customer has a new color requirement later, he only needs to tear off the original car cover, select a new car cover and re-apply it. Compared with the traditional "electrophoretic + primer + base paint + clear varnish" process, the present invention only requires basic powder coating + car cover, and the processing steps are obviously simpler and faster. Therefore, the emission of VOC (volatile organic compounds) is effectively reduced through the above method, thereby improving environmental protection benefits. At the same time, it avoids the damage to the car paint that may occur when the car cover needs to be replaced later, reduces the repair cost, and has good economic benefits. Embodiment 2
[0020] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 65kg saturated carboxylic acid polyester resin, 4.5kg TGIC curing agent, 0.2kg benzoin, 0.5kg leveling agent, and 30kg pigments and fillers; The leveling agent is ESTRON PL200; the pigment and filler are composed of barium sulfate and titanium dioxide; the mass ratio of the barium sulfate to titanium dioxide is 10:0.5; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a base powder coating with an average particle size of 28-40 μm. Embodiment 3
[0021] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 70kg saturated carboxylic acid polyester resin, 5.4kg TGIC curing agent, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a base powder coating with an average particle size of 40-50 μm. Embodiment 4
[0022] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 80kg saturated carboxylic acid polyester resin, 4.5kg HAA curing agent, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is GLP1201; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a base powder coating with an average particle size of 30-36 μm. Embodiment 5
[0023] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 65kg saturated carboxylic acid polyester resin, 3.5kg HAA curing agent, 0.5kg benzoin, 1.1kg leveling agent, 1.0kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is BYK3933P; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a base powder coating with an average particle size of 30-38 μm. Embodiment 6
[0024] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 70kg saturated carboxylic acid polyester resin, 3.8kg HAA curing agent, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is BYK3933P; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a basic powder coating with an average particle size of 30-40 μm. Embodiment 7
[0025] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 70kg saturated hydroxyl polyester resin, 18.5kg isocyanate curing agent, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is BYK3933P; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a base powder coating with an average particle size of 35-40 μm. Embodiment 8
[0026] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 55kg saturated hydroxyl polyester resin, 12.5kg isocyanate curing agent, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a basic powder coating with an average particle size of 30-40 μm. Embodiment 9
[0027] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 62kg saturated hydroxyl polyester resin, 14.3kg isocyanate curing agent, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a basic powder coating with an average particle size of 30-40 μm. Embodiment 10
[0028] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 70kg GMA acrylic resin, 18.5kg long-chain dicarboxylic acid, 0.8kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 20kg pigment filler, and 0.4kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a basic powder coating with an average particle size of 30-40 μm. Embodiment 11
[0029] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 55kg GMA acrylic resin, 13.5kg long-chain dicarboxylic acid, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 25kg pigment filler, and 0.4kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a basic powder coating with an average particle size of 30-40 μm. Embodiment 12
[0030] This embodiment provides a method for preparing a basic powder coating, comprising the following steps: Step 1: weigh 58kg GMA acrylic resin, 15.4kg long-chain dicarboxylic acid, 1.2kg benzoin, 1.1kg leveling agent, 0.3kg auxiliary degassing agent, 25kg pigment filler, and 0.4kg powdering agent; The leveling agent is ESTRON PL200; the auxiliary degassing agent is Troy Powdermate 542DG; the pigment filler is composed of barium sulfate, titanium dioxide and carbon black; the mass ratio of barium sulfate, titanium dioxide and carbon black is 12:0.6:0.04; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A through a rotating drum to form tablets, crushing it through a crusher, and grinding it into powder through a mill; Step 5: Pass the powder through a 180-mesh sieve to obtain a basic powder coating with an average particle size of 30-40 μm. Embodiment 13
[0031] The main components of the powder coating agent are surfactant, nitrogen-containing compound and fatty acid. Alternatively, the powder coating agent can also be inorganic substances (such as metal oxides, etc.).
[0032] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A basic powder coating for a vehicle body, characterized in that The invention comprises the following raw materials in parts by weight: 55-80 parts of resin, 3-18.5 parts of curing agent, 0.2-2 parts of benzoin, 0.5-1.8 parts of leveling agent, 0-1.5 parts of auxiliary degassing agent, 10-30 parts of pigments and fillers, 0-0.5 parts of powdering agent; The resin is selected from one of saturated carboxylic acid polyester resin, saturated hydroxyl polyester resin or GMA type acrylic resin, and the curing agent is selected from one of TGIC curing agent, HAA curing agent, isocyanate curing agent or long-chain dicarboxylic acid.
2. The basic powder coating for a vehicle body according to claim 1, characterized in that The leveling agent is a polyacrylate compound loaded with gas silicon.
3. The basic powder coating for a vehicle body according to claim 2, characterized in that The auxiliary degassing agent is an amino-modified phenol urea surfactant.
4. The basic powder coating for a vehicle body according to claim 3, characterized in that The pigment and filler are composed of barium sulfate, titanium dioxide and carbon black.
5. The basic powder coating for a vehicle body according to claim 4, characterized in that The mass ratio of the barium sulfate, titanium dioxide and carbon black is (10-30):(0.5-5):(0-0.1).
6. A method for preparing a basic powder coating according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: weigh 55-80 parts of resin, 3-18.5 parts of curing agent, 0.2-2 parts of benzoin, 0.5-1.8 parts of leveling agent, 0-1.5 parts of auxiliary degassing agent, 10-30 parts of pigments and fillers, and 0-0.5 parts of powdering agent; The resin is selected from one of saturated carboxylic acid polyester resin, saturated hydroxyl polyester resin or GMA type acrylic resin, and the curing agent is selected from one of TGIC curing agent, HAA curing agent, isocyanate curing agent or long-chain dicarboxylic acid; Step 2: Mix the above raw materials in a mixing pot to obtain a mixture A; Step 3: Pour the mixture A into the feed port of the screw extruder, melt the mixture A in the heating barrel of the screw extruder, and extrude the melted mixture A through hot melt mixing and extrusion of the screw extruder to obtain a molten material A; Step 4: Cooling the melt A, tableting, crushing, and grinding it into powder; Step 5: Sieve the powder to obtain a basic powder coating with a normally distributed particle size.
7. The preparation method according to claim 6, characterized in that: The leveling agent in step 1 is a polyacrylate compound loaded with gas silicon, and the auxiliary degassing agent is an amino-modified phenol urea surfactant.
8. The preparation method according to claim 7, characterized in that: In step 5, the powder is passed through a 180-mesh sieve.
9. The preparation method according to claim 8, characterized in that: The average particle size of the base powder coating described in step 5 is 28-45 μm.
10. Use of the basic powder coating according to any one of claims 1 to 5 in automobile surface treatment, characterized in that: A layer of the basic powder coating is electrostatically sprayed on the vehicle body, and then baked and cured in a baking oven at 150-200° C. for 10-20 minutes. After curing, a car cover is pasted on the outside of the basic powder coating.
Citation Information
Patent Citations
Contamination-resisting thermosetting powder paint and preparation method thereof
CN107177300A
Electrostatic spraying glaze ink composition and preparation method thereof
CN112852219A
Special vehicle powder coating
CN114316757A