Special PU (polyurethane) varnish for buoys and preparation method thereof
Through the specific PU polyurethane varnish ratio and process, the problems of insufficient adhesion, yellowing resistance and flexibility of conventional PU polyurethane varnish in float coating are solved, and the floating float with high adhesion, yellowing resistance and light-retaining performance are achieved Special PU polyurethane varnish reduces the cost of coating.
Patent Information
- Application Number
- CN202411135515.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
The conventional and ordinary two-component PU polyurethane varnish on the market is difficult to have both the phenomenon of good plumpness, good adhesion, good yellowing resistance, good flexibility, and light and color protection. The paint film has poor toughness, easy yellowing, and paint mixture. Short use time and easy gelation, resulting in increased float coating costs.
It adopts a special PU polyurethane varnish for floats, including components A and components B. Component A is composed of synthetic fatty acid resin, ether ester solvent, adhesion accelerator, polyacrylate leveling agent and silicone leveling agent. Component B consists of n-butyl acetate, dehydrating agent and HDI yellowing-resistant aliphatic isocyanate trimer curing agent. It is prepared through specific ratios and process steps, and diluent is added to adjust the construction viscosity to form an excellent paint film.
It realizes the high flexibility, yellowing resistance, adhesion and light-retaining properties of the paint film, extends the paint usage time, reduces the cost of painting, complies with national standards, and solves the poor adhesion and fullness of conventional PU bright varnishes in the float market. Poor degree and yellowing problems.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high molecular organic compounds, in particular to a PU polyurethane varnish special for floating and a preparation method thereof. Background Art
[0002] With the continuous improvement of people's material and cultural living standards, the requirements for quality of life are getting higher and higher, and the work pressure is also increasing; fishing is a relaxing activity, you can enjoy tranquility and leisure in your spare time, relieve the pressure of work and life. Outdoor fishing can be exposed to sunlight and fresh air, which is beneficial to physical and mental health. In addition, focusing on fishing can also help relieve anxiety and stress and improve mental health. With the continuous improvement of people's living standards, people's spare-time activities are also rich and colorful. Therefore, fishing activities occupy an indispensable position in people's lives and are increasingly loved and concerned by the general public. While the float occupies an indispensable position in the products of fishing supporting tools, the coating of the float paint also brings confusion to the paint manufacturers and float factories: the conventional two-component PU polyurethane varnish film on the market is difficult to achieve the coating effects of good fullness, good adhesion, good yellowing resistance, good flexibility, light and color retention, etc., due to the poor toughness of the paint film, easy yellowing, and the short use time of the paint mixture, which is easy to gel, resulting in an increase in the coating cost of the float factory. The present invention provides a special PU polyurethane weather-resistant glossy varnish for floats and a preparation method thereof to solve the above problems. Summary of the invention
[0003] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a PU polyurethane varnish special for floating and a preparation method thereof.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] A PU polyurethane varnish specially used for floating includes component A, component B and a diluent, wherein the weight ratio of component A to component B is 100:50;
[0006] Wherein, the composition of the component A and the weight proportions of each component are:
[0007] 80-90 parts of synthetic fatty acid resin;
[0008] 5-10 parts of ether ester solvents;
[0009] Defoaming agent 0.2-0.5 parts;
[0010] Adhesion promoter 0.5-2 parts;
[0011] Polyacrylate leveling agent 0.2-0.5 parts;
[0012] Fluorocarbon modified leveling agent, dosage is 0.05-0.1 part;
[0013] Organic silicon leveling agent, dosage is 0.05-0.1 part;
[0014] 5-10 parts of ester solvent;
[0015] The composition of the second component and the weight proportions of each component are:
[0016] 50-60 parts of n-butyl acetate;
[0017] Dehydrating agent: 0.1-0.5 parts of monofunctional isocyanate;
[0018] 40-50 parts of HDI yellowing-resistant aliphatic isocyanate trimer curing agent. Preferably, the composition of the diluent and the weight proportions of each component are:
[0019] Propylene glycol methyl ether acetate 5-10 parts;
[0020] 60-70 parts of n-butyl acetate;
[0021] 20-35 parts of ethyl acetate.
[0022] Preferably, the synthetic fatty acid resin has a fineness of ≤15 microns, a solid content of 80±2%, and a hydroxyl content of 165±10 mgKOH / g, preferably Guangdong Changxing Resin 3755-80 synthetic fatty acid resin or Nupes synthetic fatty acid resin 2848;
[0023] The ether ester solvent is propylene glycol methyl ether acetate;
[0024] Adhesion promoter uses modified polyester polymer compound, which bonds with the surface of the substrate to improve the adhesion of the coating film to the substrate, and improves the physical and chemical properties of the paint film, such as the flexibility and corrosion resistance of the paint film. Shenzhen Tianyuan Chemical Co., Ltd. A-7008A adhesion promoter is preferred;
[0025] The defoamer is modified polysiloxane, which has good compatibility and defoaming properties with synthetic fatty acid resin. De fom 5300 from Deqian or BYK 141 from Germany are preferred as the modified polysilane defoamer.
[0026] Preferably, the polyacrylate leveling agent is a surface additive of polyacrylate to improve the leveling performance, preferably BYK358N or EFKA3777 acrylic leveling agent;
[0027] Fluorine-modified leveling agent is a fluorocarbon polymer leveling agent, preferably EFKA3600 or EFKNA FL3600;
[0028] The silicone modified leveling agent is polyether modified polydimethylsiloxane, preferably German BYK333 or Digao additive TEG450;
[0029] Preferably, the ester solvent is n-butyl acetate.
[0030] Preferably, the dehydrating agent is a monofunctional isocyanate, and the specific models are BF-5 of Samsung Chemical, TI of Bayer AG, BF-5 of Gas Bahn AG, etc.
[0031] HDI curing agent: HDI aliphatic isocyanate trimer curing agent has super yellowing resistance and flexibility. At the same time, it can reasonably extend the usable time and has good compatibility with synthetic fatty acid resin. Wanhua Chemical Wannate HT-100HDI curing agent or German Bayer N3390 HDI yellowing resistance curing agent is preferred.
[0032] The present invention also protects a method for preparing a PU polyurethane varnish specially used for floating.
[0033] The preparation method of the first component comprises the following steps:
[0034] Step 11: Add synthetic fatty acid resin, ether ester solvent, adhesion promoter, and defoamer into a dispersion tank for dispersion;
[0035] Step 12: in step 11, adding polyacrylate leveling agent, fluorine-modified leveling agent and organosilicon-modified leveling agent while stirring to disperse; wherein the fluorine-modified leveling agent and organosilicon-modified leveling agent are diluted with n-butyl acetate in advance and stirred evenly, and then added while stirring;
[0036] Step 13: Add an ester solvent to the qualified slurry obtained in step 12, disperse it until it is uniform, and then filter and package it after passing the inspection;
[0037] The method for preparing the second component comprises the following steps: adding a dehydrating agent into n-butyl acetate solvent, allowing it to fully dehydrate for 24 hours, and then sequentially adding HDI curing agent and fully stirring.
[0038] Preferably, in step 11, the dispersion is carried out at a speed of 600-800 rpm for 5-8 minutes until uniform;
[0039] In the step 12, the dispersion is carried out at a speed of 1200-1500 rpm for 15-25 minutes, and the fineness is ≤20 um;
[0040] In the step 13, the dispersion is carried out at a speed of 600-800 rpm for 5-10 minutes.
[0041] The present invention also protects a method for using a PU polyurethane varnish specially used for floating, which comprises mixing component A and component B in a weight fraction ratio of 100:50, adding a diluent, and adjusting the viscosity to a suitable construction viscosity before construction. After drying, a paint film with excellent physical and chemical properties and decorative properties can be obtained.
[0042] The PU polyurethane varnish for floating of the present invention has the following beneficial effects:
[0043] 1. High hydroxyl synthetic fatty acid resin is introduced to ensure that the paint film has good fullness and flexibility after drying. In addition to the high fullness of traditional alkyd resin, high hydroxyl synthetic fatty acid resin also has excellent super yellowing resistance, adhesion and gloss retention, thus achieving permanent yellowing resistance, gloss retention and high flexibility.
[0044] 2. Use special additives and adhesion promoters, which are special modified polyester polymer compounds. They can bond with the surface of the substrate, improve the adhesion of the coating to the substrate, and improve the physical and chemical properties of the paint film, such as the flexibility and corrosion resistance of the paint film. This additive can have good adhesion to the floating substrate and improve the fullness of the paint film. Therefore, the paint has good fullness, good adhesion and good flexibility after film formation.
[0045] 3. The HDI super yellowing-resistant aliphatic isocyanate trimer curing agent in the second component, which has good compatibility with the synthetic fatty acid resin, is reasonably matched to ensure that the surface drying and actual drying processes of the coating are reasonably controlled, while at the same time extending the usable time of the mixed oil and making the paint film have good fullness, super yellowing resistance and high flexibility, thus achieving the purpose of a paint film that is both super yellowing-resistant and anti-cracking and peeling. DETAILED DESCRIPTION
[0046] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0047] Component A and Component B are respectively proportioned according to the components in Table 1 and Table 2 to obtain Examples 1 to 6. Table 1 - Proportion table of Component A Examples 1 to 6
[0048]
[0049]
[0050] The preparation method of the above component A embodiment is:
[0051] Step 11: First add items 1 to 4 into the dispersion tank, and disperse at a speed of 600-800 rpm for about 5-8 minutes until uniform.
[0052] Step 12: After adding items 5 to 7 in step 11, disperse at a speed of 1200-1500 rpm for 15-25 minutes until the fineness is ≤20um. EFKA3600 and BYK333 are diluted with n-butyl acetate in advance and stirred evenly, then added while stirring.
[0053] Step 13: Add item 8 to the qualified slurry obtained in step 12, stir at a speed of 600-800 rpm for about 5-10 minutes until it is uniformly tested and qualified, then filter and package.
[0054] Table 2 - Proportion table of component B embodiments 1-6
[0055]
[0056]
[0057] The preparation method of component B is:
[0058] Step 21: Mix items 1 and 2 thoroughly and leave them for 24 hours to fully dehydrate.
[0059] Step 22: Add item 3 to the solvent prepared in step 21 in order, stir well and filter with 300-mesh filter cloth before packaging.
[0060] Mix component A and component B prepared by the above method in a weight ratio of 100:50, add an appropriate amount of diluent to adjust to the corresponding construction viscosity, and then spray test:
[0061] (1) The above Examples 1-6 (Component A) and Examples 1-6 (Component B) are matched in a one-to-one manner, that is, Example 1 of Component A is mixed with Example 1 of Component B, and Example 2 of Component A is mixed with Example 2 of Component B. The performance test results are shown in Tables 3 and 4:
[0062] Table 3
[0063]
[0064]
[0065] Table 4
[0066]
[0067]
[0068] (2) When the component A of Examples 1-4 is mixed with any one of the component B of Examples 1-4 (such as Example 1) at a ratio of 100:50, the performance test results are compared with those of conventional PU glossy varnish and competitive product samples as shown in Tables 5 and 6:
[0069] Table 5
[0070]
[0071]
[0072] Table 6
[0073]
[0074] The test results in Table 5 and Table 6 show that the introduction of high hydroxyl synthetic fatty acid resin ensures that the paint film has good fullness and flexibility after drying. In addition to the high fullness of traditional alkyd resin, high hydroxyl synthetic fatty acid resin also has excellent super yellowing resistance, adhesion and gloss retention, thereby achieving permanent yellowing resistance, gloss retention and high flexibility. The special additive adhesion promoter is a special modified polyester polymer compound that can bond with the surface of the substrate, improve the adhesion of the coating film to the substrate, and improve the physical and chemical properties of the paint film, such as the flexibility and corrosion resistance of the paint film. This additive can have good adhesion to the floating substrate and improve the fullness of the paint film, so the paint has good fullness, good adhesion and good flexibility after film formation. The HDI super yellowing-resistant aliphatic isocyanate trimer curing agent in the second component, which has good solubility with the synthetic fatty acid resin, is reasonably matched, so that the time of the surface drying and actual drying of the coating film can be reasonably controlled, and at the same time the usable time of the mixed oil can be extended, and the paint film has a good fullness, super yellowing resistance and high flexibility, thus achieving the purpose of a paint film effect that is both super yellowing-resistant and anti-cracking and peeling.
[0075] The invention complies with the national standards GB18581-2020 and GB / T23997-2009, and solves the problems of poor adhesion of the paint film of ordinary two-component PU glossy varnish polyurethane coatings in the float market, poor fullness, yellowing in the later period, bending and cracking of the float, and short usable time. At the same time, it has excellent adhesion and flexibility, and good gloss and color retention properties, and the comprehensive performance of the paint film is excellent.
[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A PU polyurethane varnish for floating, characterized in that : comprising component A, component B and a diluent, wherein the weight ratio of the component A to the component B is 100:50; Wherein, the composition of the component A and the weight proportions of each component are: 80-90 parts of synthetic fatty acid resin; 5-10 parts of ether ester solvents; Defoaming agent 0.2-0.5 parts; Adhesion promoter 0.5-2 parts; Polyacrylate leveling agent 0.2-0.5 parts; Fluorocarbon modified leveling agent, dosage is 0.05-0.1 part; Organic silicon leveling agent, dosage is 0.05-0.1 part; 5-10 parts of ester solvent; The composition of the second component and the weight proportions of each component are: 50-60 parts of n-butyl acetate; Dehydrating agent 0.1-0.5 parts; 40-50 parts of curing agent.
2. A PU polyurethane varnish for floating according to claim 1, characterized in that: The composition of the diluent and the weight proportions of each component are: Propylene glycol methyl ether acetate 5-10 parts; 60-70 parts of n-butyl acetate; 20-35 parts of ethyl acetate.
3. A PU polyurethane varnish for floating according to claim 1, characterized in that: The synthetic fatty acid resin has a fineness of ≤15 microns, a solid content of 80±2%, and a hydroxyl content of 165±10 mgKOH / g; The ether ester solvent is propylene glycol methyl ether acetate; The adhesion promoter is a modified polyester polymer compound that bonds to the surface of the substrate; The defoaming agent is modified polysiloxane, which has good compatibility and defoaming properties with synthetic fatty acid resin.
4. A PU polyurethane varnish for floating according to claim 1, characterized in that: The polyacrylate leveling agent is a surface additive of polyacrylate to improve the leveling performance; The fluorine-modified leveling agent is a fluorocarbon polymer leveling agent; The organosilicon-modified leveling agent is polyether-modified polydimethylsiloxane.
5. A PU polyurethane varnish for floating according to claim 1, characterized in that: The ester solvent is selected from n-butyl acetate.
6. A PU polyurethane varnish for floating according to claim 1, characterized in that: The dehydrating agent is a monofunctional isocyanate.
7. The PU polyurethane varnish for floating according to claim 1, characterized in that: The curing agent is HDI aliphatic isocyanate trimer curing agent.
8. A method for preparing a PU polyurethane varnish for floating according to any one of claims 1 to 7, characterized in that: The preparation method of the first component comprises the following steps: Step 11: Add synthetic fatty acid resin, ether ester solvent, adhesion promoter, and defoamer into a dispersion tank for dispersion; Step 12: in step 11, adding polyacrylate leveling agent, fluorine-modified leveling agent and organosilicon-modified leveling agent while stirring to disperse; wherein the fluorine-modified leveling agent and organosilicon-modified leveling agent are diluted with n-butyl acetate in advance and stirred evenly, and then added while stirring; Step 13: Add an ester solvent to the qualified slurry obtained in step 12, disperse it until it is uniform, and then filter and package it after passing the inspection; The method for preparing the second component comprises the following steps: adding a dehydrating agent into n-butyl acetate solvent, allowing it to fully dehydrate for 24 hours, and then sequentially adding HDI curing agent and fully stirring.
9. The method for preparing a PU polyurethane varnish for floating according to claim 8, characterized in that: In the step 11, the mixture is dispersed at a speed of 600-800 rpm for 5-8 minutes until uniform; In the step 12, the dispersion is carried out at a speed of 1200-1500 rpm for 15-25 minutes, and the fineness is ≤20 um; In the step 13, the dispersion is carried out at a speed of 600-800 rpm for 5-10 minutes.
10. The method for using the PU polyurethane varnish for floating according to any one of claims 1 to 7, characterized in that: Mix component A and component B in a weight fraction ratio of 100:50, add diluent, and adjust to a suitable construction viscosity before construction. After drying, a paint film with excellent physical and chemical properties and decorative properties can be obtained.
Citation Information
Patent Citations
Furniture coating
CN106833363A
High solid content odorless polyurethane varnish
CN107858090A
Technical wood special polyurethane paint and preparation method thereof
CN109486407A
Two-component polyurethane yellowing-resistant high-gloss finish paint for melamine coated cabinet and preparation method thereof
CN111548724A
High-weather-resistance and anti-yellowing coating and preparation method thereof
CN115785786A