UV wiredrawing finish paint for vacuum coating as well as preparation method and application of UV wiredrawing finish paint
By using fluorocarbon modified and nano-modified UV polyurethane resin in UV brushed topcoat for vacuum coating, the problems of existing coatings in poor anti-glare, graffiti resistance and wear resistance are solved, and high-performance coatings are achieved The layer effect meets the dual requirements of electronic products for thin coating properties and hardness.
Patent Information
- Application Number
- CN202411005843.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing wear-resistant matte UV coatings cannot meet the thin coating requirements of electronic products for anti-glare, graffiti resistance and high wear resistance, especially when the paint film is less than 10 microns.
UV brushed topcoat for vacuum coating is adopted, and the formula includes fluorocarbon modified UV polyurethane resin, polyurethane acrylic resin and nano-modified UV polyurethane resin. Through the characteristics of these materials, the coating is improved by improving the heat resistance, chemical corrosion resistance and graffiti resistance of the coating. and anti-glare properties and rapidly cure through photoinduced polymerization reaction to form a hard transparent coating.
It achieves excellent steel wool resistance, graffiti resistance and anti-glare effects, improves the hardness and toughness of the coating, reduces material waste and production costs, and ensures high-quality paint film performance.
Smart Images

Figure BDA0004962990240000091 
Figure BDA0004962990240000101 
Figure BDA0004962990240000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a UV drawing topcoat for vacuum coating, a preparation method and an application thereof. Background Art
[0002] Modern industrial coating is one of the most important process links in the manufacturing industry. It plays an extremely important role in improving the commodity and decorative properties of products, extending the service life of products and providing special functions. With the substantial increase in the use and frequency of mobile online office, mobile online education and new energy vehicles, the comprehensive user experience of the anti-glare effect, graffiti resistance, high wear resistance and feel of electronic products is getting higher and higher. As electronic products and vehicles are becoming thinner and lighter, the requirements for paint films are also getting higher and higher. When the paint film is less than 10 microns, the above requirements must be met while taking into account the guarantee of flexibility and hardness, so high requirements are placed on the quality of the coating. The existing ordinary wear-resistant matte UV cannot meet the thin coating properties of AG coatings, and the anti-glare and wear resistance of the coating are poor.
[0003] Therefore, there is an urgent need for a UV brushed topcoat coating for vacuum coating with good anti-glare effect. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a UV brushed topcoat for vacuum coating and a preparation method and application thereof to solve the problems of poor steel wool resistance, graffiti resistance and anti-glare effect.
[0005] The present invention also provides a method for preparing the UV wire drawing topcoat for vacuum coating.
[0006] The present invention also proposes the application of the above-mentioned UV wire drawing topcoat for vacuum coating in the housing of electronic products.
[0007] According to one aspect of the present invention, a UV brushed topcoat for vacuum coating is provided. The raw materials for preparation include, by weight: 20 to 30 parts of fluorocarbon modified UV polyurethane resin, 10 to 20 parts of polyurethane acrylic resin, and 20 to 30 parts of nano-modified UV polyurethane resin.
[0008] According to the embodiments of the first aspect of the present invention, there are at least the following beneficial effects:
[0009] The UV topcoat of the present invention has excellent steel wool resistance, graffiti resistance and anti-glare effects; wherein the fluorocarbon group of the fluorocarbon modified UV polyurethane resin provides super hydrophobicity for the coating, enhances the anti-graffiti and anti-fingerprint properties, can reduce the surface tension of the paint film, and improves the excellent properties of the paint film such as heat resistance and chemical corrosion resistance. The polyurethane group has good wear resistance and flexibility, so that the coating has high wear resistance and good physical properties.
[0010] The nanoparticles of nano-modified UV polyurethane resin reduce shrinkage by restricting the movement of polymer chains during the curing process, form functional groups that form chemical bonds with the resin matrix, improve adhesion, enhance the bond between the resin and the metal substrate, absorb impact energy, promote plastic deformation or prevent crack propagation to improve toughness, increase the hardness of the coating, and reduce wear.
[0011] In some embodiments of the present invention, the polyurethane acrylic resin includes a 9-15 functional polyurethane acrylic resin.
[0012] The above-mentioned 9-15 functional polyurethane acrylic resin has a large number of functional groups and a relatively short chain length; it has a high hardness, thereby improving the wear resistance of the paint film.
[0013] The addition of acrylic polyurethane wax slurry and matting powder can improve the wear resistance of the coating. At the same time, the microcrystalline structure of the wax helps to scatter light and increase the anti-glare effect of the coating.
[0014] Promotes fast curing: In UV-curable coatings, the multifunctional nature of DPEHA enables it to quickly form a hard and transparent coating through photoinitiated polymerization
[0015] In some embodiments of the present invention, the fluorocarbon modified UV polyurethane resin includes Lancolu L-6905B.
[0016] In some embodiments of the present invention, the fluorocarbon modified UV polyurethane resin has a solid content of 98%, a viscosity of 15000-25000 cps / 25° C., and an acid value of 1 mgKOH / g.
[0017] In some embodiments of the present invention, the nano-modified UV polyurethane resin has a solid content of 90% and a viscosity of 1000-2000 cps / 25°C.
[0018] High solid content can reduce the amount of solvent used, improve the thickness and quality of the coating. Appropriate viscosity facilitates processing, improves the uniformity of the coating, improves construction performance, etc. High solid content and appropriate viscosity help reduce material waste, improve material utilization, and thus reduce production costs.
[0019] In some embodiments of the present invention, the nano-modified UV polyurethane resin includes UA-895 produced by Zhongshan JST.
[0020] In some embodiments of the present invention, the polyurethane acrylic resin includes 6196-100 of Changxing Chemical.
[0021] In some embodiments of the present invention, the acrylic polyurethane wax slurry includes BG-06 from Gifu, Japan.
[0022] In some embodiments of the present invention, the dispersant includes BYK110 polymerized phosphate solution.
[0023] In some embodiments of the present invention, the photoinitiator includes at least one of Irgacure 184 and Darocur TPO from JIURI.
[0024] In some embodiments of the present invention, the raw materials for preparing the UV brushed topcoat for vacuum coating further include an auxiliary agent;
[0025] The auxiliary agent comprises acrylic polyurethane wax slurry, matting powder, photoinitiator, dispersant, diluent and leveling agent.
[0026] The wax in acrylic polyurethane wax paste has a microcrystalline structure that helps scatter light and increase the anti-glare effect of the coating.
[0027] In some embodiments of the present invention, the raw materials for preparing the UV brushed topcoat for vacuum coating further include aliphatic polyurethane resin.
[0028] In some embodiments of the present invention, the raw materials for preparing the UV brushed topcoat for vacuum coating further include a hexafunctional monomer, and the hexafunctional monomer includes dipentaerythritol hexaacrylate.
[0029] The dipentaerythritol hexaacrylate in the present invention has six acrylic acid functional groups, can quickly react with a variety of monomers or polymers through photoinitiated polymerization to form a three-dimensional network structure, and has high reactivity.
[0030] In some embodiments of the present invention, the diluent includes at least one of methyl isobutyl ketone and diacetone alcohol and butyl acetate.
[0031] In some embodiments of the present invention, the diluent includes methyl isobutyl ketone and diacetone alcohol and butyl acetate.
[0032] In some embodiments of the present invention, the diluent includes, by weight, 9 to 12 parts of methyl isobutyl ketone, 8 to 12 parts of diacetone alcohol, and 9 to 15 parts of butyl acetate.
[0033] The diluent in the above weight proportion helps to improve the performance stability and water resistance of the final product.
[0034] In some embodiments of the present invention, the preparation raw materials include, by weight: 20 to 30 parts of fluorocarbon modified UV polyurethane resin, 10 to 20 parts of polyurethane acrylic resin, 20 to 30 parts of nano-modified UV polyurethane resin, 10 parts of aliphatic polyurethane resin, 5 to 8 parts of acrylic polyurethane wax slurry, 5 to 7 parts of matting powder, 3 to 5 parts of photoinitiator, 1 to 2 parts of dispersant, 20 to 30 parts of diluent and 0.5 to 10 parts of leveling agent.
[0035] In some embodiments of the present invention, the preparation raw materials include, by weight: 20 to 30 parts of fluorocarbon modified UV polyurethane resin, 10 to 20 parts of polyurethane acrylic resin, 20 to 30 parts of nano-modified UV polyurethane resin, 10 parts of aliphatic polyurethane resin, 5 to 8 parts of acrylic polyurethane wax slurry, 5 to 7 parts of matting powder, 5 to 6 parts of hexafunctional monomer, 3 to 5 parts of photoinitiator, 1 to 2 parts of dispersant, 20 to 30 parts of diluent and 0.5 to 10 parts of leveling agent.
[0036] In some embodiments of the present invention, the leveling agent includes polyether-modified polydimethylsiloxane.
[0037] According to two aspects of the present invention, a method for preparing a wire drawing topcoat is provided, comprising: mixing and reacting raw materials for preparing the vacuum coating UV wire drawing topcoat.
[0038] In some embodiments of the present invention, the method for preparing the wire drawing topcoat comprises:
[0039] S1. Preheating the polyurethane acrylic resin, nano-modified UV polyurethane resin, and fluorocarbon-modified UV polyurethane resin to obtain a premix 1;
[0040] S2. The photoinitiator is added to part of the diluent to obtain a premix 2;
[0041] S3. Add premix 2 to premix 1 and mix;
[0042] S4. Add the hexafunctional monomer, dispersant, matting powder, acrylic polyurethane wax slurry, leveling agent and remaining diluent into step S3 and mix them to obtain the UV brushed topcoat for vacuum coating.
[0043] In some embodiments of the present invention, step S3 further includes filtering after the mixing.
[0044] This can further improve the mixing uniformity of the UV brushed topcoat for vacuum coating and remove large particle impurities therein.
[0045] According to three aspects of the present invention, a composite coating is provided, the composite coating comprising a primer layer, an electroplating film layer, a mid-coat layer and a topcoat layer stacked in sequence;
[0046] The raw materials for preparing the topcoat layer include the UV drawing topcoat for vacuum coating.
[0047] In some embodiments of the present invention, the setting method includes:
[0048] D1. Spray the treatment agent on the surface of the substrate and obtain the treatment agent coating after leveling;
[0049] D2. spraying a primer on the surface of the treatment agent coating, and leveling and curing to obtain the primer layer;
[0050] D3 NCVM electroplating is performed on the surface of the primer layer to obtain the plated film layer;
[0051] D4. Spraying the middle paint on the middle paint layer, leveling and curing to obtain the middle paint layer;
[0052] D5. spraying the obtained vacuum coating on the surface of the intermediate paint layer, leveling it with UV brushed topcoat, and performing light curing to obtain the topcoat layer.
[0053] In some embodiments of the present invention, in step D1, the leveling temperature is 50-60°C.
[0054] In some embodiments of the present invention, the leveling temperature is 53°C, 55°C or 57°C.
[0055] In some embodiments of the present invention, in step D1, the leveling time is 5 to 15 minutes.
[0056] In some embodiments of the present invention, the leveling time is 6 min, 7 min, 8 min, 10 min or 12 min.
[0057] In some embodiments of the present invention, in step D1, the material of the substrate includes at least one of polycarbonate and acrylonitrile-butadiene-styrene plastic.
[0058] In some embodiments of the present invention, in step D2, the leveling temperature is 50-60°C.
[0059] In some embodiments of the present invention, in step D2, the leveling temperature is 53°C, 55°C or 57°C.
[0060] In some embodiments of the present invention, in step D2, the leveling time is 5 to 15 minutes.
[0061] In some embodiments of the present invention, in step D2, the leveling time is 6 min, 8 min, 10 min or 12 min.
[0062] In some embodiments of the present invention, in step D2, the curing method includes photocuring.
[0063] In some embodiments of the present invention, the energy of the light used for photocuring is 700-900 mJ / cm 2 .
[0064] In some embodiments of the present invention, in step D3, the target material for NCVM electroplating includes indium.
[0065] In some embodiments of the present invention, in step D4, the leveling temperature is 50-60°C.
[0066] In some embodiments of the present invention, in step D4, the leveling temperature is 52°C, 55°C or 58°C.
[0067] In some embodiments of the present invention, in step D4, the leveling time is 5 to 15 minutes.
[0068] In some embodiments of the present invention, in step D4, the leveling time is 6 min, 8 min, 10 min or 12 min.
[0069] In some embodiments of the present invention, in step D4, the energy of the light used for photocuring is 800-1000 mJ / cm 2 .
[0070] In some embodiments of the present invention, in step D4, the energy of the light used for photocuring is 850 mJ / cm 2 、900mJ / cm 2 or 950mJ / cm 2 .
[0071] According to some embodiments of the present invention, in step D5, the leveling temperature is 50-70°C.
[0072] According to some embodiments of the present invention, in step D5, the leveling temperature is 55°C, 60°C or 65°C.
[0073] According to some embodiments of the present invention, in step D5, the leveling time is 5 to 15 minutes.
[0074] According to some embodiments of the present invention, in step D5, the leveling time is 7 min, 10 min or 12 min.
[0075] According to some embodiments of the present invention, in step D5, the curing method is photocuring.
[0076] According to some embodiments of the present invention, in step D5, the energy of the light used for photocuring is 800-1000 mJ / cm 2 .
[0077] According to some embodiments of the present invention, in step D5, the energy of the light used for photocuring is 800 mJ / cm 2 、900mJ / cm 2 or 1000mJ / cm2 .
[0078] In some embodiments of the present invention, the composite coating further includes a treatment agent coating disposed on a surface of the primer layer away from the electroplating film layer.
[0079] In some embodiments of the present invention, the thickness of the treatment agent coating is 10 to 20 μm.
[0080] In some embodiments of the present invention, the thickness of the treatment agent coating is 13 μm, 15 μm or 17 μm.
[0081] Unless otherwise specified, the coating thicknesses defined in the present invention are all dry film thicknesses.
[0082] According to some embodiments of the present invention, the primer layer has a thickness of 20 to 30 μm.
[0083] According to some embodiments of the present invention, the thickness of the primer layer is 23 μm, 25 μm or 27 μm.
[0084] According to some embodiments of the present invention, the thickness of the electroplated film layer is 20-30 nm.
[0085] According to some embodiments of the present invention, the thickness of the primer layer is 23 nm, 25 nm or about 27 nm.
[0086] According to some embodiments of the present invention, the material of the electroplated film layer includes indium.
[0087] According to some embodiments of the present invention, the thickness of the middle paint layer is 4-8 μm.
[0088] According to some embodiments of the present invention, the thickness of the middle paint layer is 5 μm, 6 μm or 7 μm.
[0089] According to some embodiments of the present invention, the thickness of the topcoat layer is 6-10 μm.
[0090] According to some embodiments of the present invention, the thickness of the topcoat layer is 6 μm, 8 μm or 10 μm.
[0091] According to an embodiment of the present invention, a method for setting the composite coating is provided, the method comprising spraying the vacuum coating UV brushed topcoat onto the surface of the intermediate paint layer, leveling the topcoat, and performing photocuring to obtain the topcoat layer.
[0092] According to four aspects of the present invention, an application of the composite coating in an electronic product housing is proposed.
[0093] According to some embodiments of the present invention, the electronic product includes at least one of a smart phone, a notebook, a mobile camera and a smart wearable device.
[0094] In some embodiments of the present invention, the paint film of the electronic product housing is not higher than 10 μm. DETAILED DESCRIPTION
[0095] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.
[0096] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0097] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0098] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0099] Unless otherwise specified, the sources of some raw materials used in the specific implementation methods are summarized as follows:
[0100] The nano-modified UV polyurethane resin is UA-895 produced by Zhongshan JST.
[0101] The nano hybrid polyurethane resin is Lancolu L-6905B;
[0102] The polyurethane acrylic resin is 6196-100 from Changxing Chemical;
[0103] The aliphatic polyurethane resin is 266;
[0104] The dipentaerythritol hexaacrylate is DPHA from Changxing Chemical;
[0105] The acrylic polyurethane wax paste was purchased from Gifu, Japan, BG-06;
[0106] The dispersant is BYK110 polymerized phosphate solution;
[0107] The leveling agent is BYK 333 polyether modified polydimethylsiloxane;
[0108] The photoinitiator is Irgacure 184 and / or Darocur TPO from Jiuri Company;
[0109] The treatment agent is Matsui's PAP30737;
[0110] The primer is Matsui’s PEB10060 A;
[0111] The midcoat is Matsui's SP120-20013-1.
[0112] In order to further understand the working principle and effective technical effects of the present invention, embodiments are provided below for illustration.
[0113] Example 1
[0114] In this example, a UV brushed topcoat for vacuum coating was prepared. The raw material ratio is shown in Table 1. The specific steps are as follows:
[0115] S1. Preheating the polyurethane acrylic resin, the nano-modified UV polyurethane resin, and the nano-hybrid polyurethane resin to obtain a premix 1;
[0116] S2. The photoinitiator is added to part of the diluent to obtain a premix 2;
[0117] S3. Add premix 2 to premix 1 and mix;
[0118] S4. Add dipentaerythritol hexaacrylate, dispersant, matting powder, acrylic polyurethane wax slurry, leveling agent and remaining diluent into step S3 and mix to obtain the UV brushed topcoat for vacuum coating.
[0119] Embodiments 2 to 6
[0120] Examples 2 to 6 respectively prepare a UV brushed topcoat for vacuum coating, and the specific difference from Example 1 is that the amounts of some preparation raw materials are different, and the specific amounts are shown in Table 1.
[0121] For ease of presentation, two tables are used below to express the proportions of the embodiments and their product performances, namely Table 1: Weight percentages of the raw materials for preparing the UV brushed topcoat in the embodiments; Table 2: Performance test results of the UV brushed topcoat prepared based on the proportions of the embodiments.
[0122] Comparative Example 1
[0123] In this comparative example, a UV brushed topcoat for vacuum coating is prepared. The difference between this comparative example and Example 1 is that butyl acetate is used to replace the dipentaerythritol hexaacrylate in Example 1, and the other conditions are the same.
[0124] Comparative Example 2
[0125] In this comparative example, a UV brushed topcoat for vacuum coating is prepared. The difference between this comparative example and Example 1 is that the nano-modified UV polyurethane resin and the fluorocarbon-modified UV polyurethane resin in Example 1 are replaced by polyurethane acrylic resin, and the other conditions are the same.
[0126] Comparative Example 3
[0127] In this comparative example, a UV brushed topcoat for vacuum coating is prepared. The difference between this comparative example and Example 1 is that the acrylic polyurethane wax slurry in Example 1 is replaced by silica matting powder, and the other conditions are the same.
[0128] Table 1. Weight percentage of raw materials for preparing UV wire drawing topcoat in the embodiment
[0129]
[0130]
[0131] Test Case
[0132] In this test example, the UV brushed topcoat for vacuum coating obtained in the embodiment was used as part of the raw materials to prepare a composite coating for the middle frame of a mobile phone. The specific process is as follows:
[0133] D1. Spray the treatment agent onto the substrate (PC material) with a spray film thickness of 15 μm, and level it at 60°C for 10 minutes to obtain a treatment agent coating loaded on the surface of the substrate;
[0134] D2. Spray the primer onto the surface of the treatment agent coating with a film thickness of 30 μm and level it at 60°C for 10 minutes; use an arm length range of 200 to 450 nm and an energy of 800 mJ / cm 2 The primer layer is obtained by light curing;
[0135] D3. NCVM electroplating was performed on the primer layer, the electroplating target was indium, and a plated film layer with a thickness of 25 nm was obtained;
[0136] D4. Spray the intermediate paint on the electroplated film layer with a film thickness of 8μm and level it at 55℃ for 10min; and use 1000mJ / cm 2 Energy photocuring, the wavelength range of the light used is 200-450nm; a middle paint layer is obtained;
[0137] D5. The UV brushed topcoat for vacuum coating obtained in the embodiment was sprayed on the middle paint layer, with a spray film thickness of 8 μm, and leveled at 65° C. for 10 min; and cured with energy light, the wavelength range of the light used was 200 to 450 nm; to obtain a topcoat layer.
[0138] Table 2. Performance test results of UV brushed topcoat prepared based on the ratio of the embodiment
[0139]
[0140] The paint film thickness of the embodiment is controlled at 6-10 microns, and the specific indicators of the performance test include:
[0141] 1. The graffiti resistance test means using a ZEBRA (oily pen) to draw three 3cm long marks on the surface of the paint film. After leaving it for 10 minutes, wipe it with a dust-free cloth. If there is no trace of the oil pen remaining, it is qualified.
[0142] 2. Steel wool test refers to using No. 0000 steel wool with a load of 1000g, a stroke of 20mm*20mm, a speed of 1s / time, and a back and forth test for 2000 times. Then wipe the test part with a dust-free cloth dipped in alcohol and observe the scratch level of the test part surface. 0-2 levels are qualified. Check the sample surface before testing, test the sample gloss (transparent parts need to test the transmittance of the sample). Compared with the gloss before wear resistance, the change in value should be less than 5% to pass.
[0143] 3. The bending test means that the sample is sprayed with the surface facing outwards, and the sample is bent 180 degrees on a cylindrical axis of a certain diameter at the same position. The bending should be completed within 1-2 seconds. The diameters of the cylinders are 20, 16, 14, 12, and 10 mm respectively. The paint film after bending is qualified if there are no cracks on its appearance.
[0144] 4. The haze test is to place the sample on the test bench of the haze meter, and use the reading displayed by the instrument as the judgment result to evaluate the anti-glare performance of the coating. The higher the haze value, the better the anti-glare effect. A higher haze means that the material has a stronger ability to scatter light, which helps to reduce glare.
[0145] Comparison of Example 1 with Comparative Example 1 shows that the curing speed is significantly improved by adding dipentaerythritol hexaacrylate.
[0146] By comparing Example 1 with Comparative Example 2, it can be seen that by adding polyurethane acrylic resin to replace the nano-modified UV polyurethane resin and fluorocarbon-modified UV polyurethane resin in Example 1, the steel wool resistance performance is significantly reduced, and the graffiti resistance effect is significantly reduced.
[0147] Comparison between Example 1 and Comparative Example 3 shows that the anti-glare effect is significantly reduced by adding silicon dioxide matting powder to replace the acrylic polyurethane wax paste in Example 1.
[0148] Comparison between Example 1 and Example 2 shows that the addition of aliphatic polyurethane resin significantly reduces the steel wool resistance and graffiti resistance.
[0149] Comparison between Example 1 and Example 7 shows that the addition of the mixed solvent significantly improves the stability and water resistance of the paint film.
[0150] Comparing Example 2 with Example 3, it can be seen that: when the acrylic polyurethane wax slurry is less than 3%, it will be significantly worse, and when it reaches 5%, the hand feel is smoother, and the graffiti resistance effect has no residue; compared with Example 6, the hand feel is obviously rougher and the paint film has particles, and the gloss is significantly improved after the steel wool test. The surface of the filler has a low friction coefficient, which creates a smooth touch on the surface of the material. The microstructure of the acrylic polyurethane wax slurry is similar to the lotus leaf effect in nature, with a roughness at the micron or nanometer level, which can reduce the direct contact area and thus reduce friction. The filler is evenly dispersed in the substrate and can form a uniform coating on the surface of the material, improving the consistency and smoothness of the hand feel.
[0151] Comparison between Example 3 and Example 4 and Example 5 shows that when the polyurethane acrylic resin reaches 20%, the flexibility of the paint film is significantly deteriorated; when the nano-modified UV polyurethane resin is less than 30%, the wear resistance and gloss of the steel wool are significantly improved.
[0152] It can be seen that the vacuum-coated UV brushed topcoat has good steel wool and graffiti resistance, good anti-glare effect, fast curing speed, can be shipped directly without baking, low energy consumption, high production efficiency, high paint film hardness, and resistance to high temperature and humidity.
[0153] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection of the technical solution of the present invention.
Claims
1. A UV brushed topcoat for vacuum coating, characterized in that: The raw materials include, by weight: 20 to 30 parts of fluorocarbon modified UV polyurethane resin, 10 to 20 parts of polyurethane acrylic resin, and 20 to 30 parts of nano-modified UV polyurethane resin.
2. The UV brushed topcoat for vacuum coating according to claim 1, characterized in that: The raw materials for preparing the UV wire drawing topcoat for vacuum coating also include auxiliary agents; The auxiliary agent comprises acrylic polyurethane wax slurry, matting powder, photoinitiator, dispersant, diluent and leveling agent.
3. The UV drawing topcoat for vacuum coating according to claim 2, characterized in that: The raw materials for preparing the UV brushed topcoat for vacuum coating also include aliphatic polyurethane resin; preferably, the raw materials for preparing the UV brushed topcoat for vacuum coating also include hexafunctional monomers, and the hexafunctional monomers include dipentaerythritol hexaacrylate.
4. The UV drawing topcoat for vacuum coating according to claim 2, characterized in that: The diluent includes at least one of methyl isobutyl ketone, diacetone alcohol and butyl acetate.
5. The UV drawing topcoat for vacuum coating according to claim 4, characterized in that: The diluent comprises methyl isobutyl ketone, diacetone alcohol and butyl acetate; preferably, by weight, the diluent comprises: 9 to 12 parts of methyl isobutyl ketone, 8 to 12 parts of diacetone alcohol and 9 to 15 parts of butyl acetate.
6. The UV drawing topcoat for vacuum coating according to claim 3, characterized in that: The raw materials include, by weight: 20-30 parts of fluorocarbon modified UV polyurethane resin, 10-20 parts of polyurethane acrylic resin, 20-30 parts of nano-modified UV polyurethane resin, 10 parts of aliphatic polyurethane resin, 5-8 parts of acrylic polyurethane wax slurry, 5-7 parts of matting powder, 3-5 parts of photoinitiator, 1-2 parts of dispersant, 20-30 parts of diluent and 0.5-10 parts of leveling agent.
7. The UV drawing topcoat for vacuum coating according to claim 2, characterized in that: The leveling agent includes polyether-modified polydimethylsiloxane.
8. The method for preparing the UV drawing topcoat for vacuum coating according to any one of claims 1 to 7, characterized in that: include: The raw materials for preparing the vacuum coating and UV wire drawing topcoat are mixed and reacted.
9. A composite coating, characterized in that: The composite coating comprises a primer layer, an electroplating film layer, a mid-coat layer and a topcoat layer which are stacked in sequence; The raw materials for preparing the topcoat layer include the UV drawing topcoat for vacuum coating according to any one of claims 1 to 7.
10. Use of the composite coating according to claim 9 in an electronic product housing.
Citation Information
Patent Citations
High-hardness, high-wear-resistant and anti-fingerprint ultraviolet-curable coating
CN109536001A
Anti-dazzle anti-fingerprint wear-resistant hardening liquid with rubber hand feeling, and preparation method thereof
CN113683952A
Non-stick UV coating as well as preparation method and application thereof
CN117586658A
Multi-Functional Hard Coating Composition And Hard Coating Structure
KR1020110035356A
Cited By
Frame body surface treatment method, frame body and electronic equipment
CN119281625A