Coating applique with reduced defects, articles and methods

Through in-situ polymerization, defect-free colored polymer films and multi-layer structures, the adhesion and removal problems of coating replacement technology in the transportation industry are solved, and the durability and aesthetics of coating decals are improved. It is suitable for composite material surfaces .

CN118909561APending Publication Date: 2024-11-08PPG ADVANCED SURFACE TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222570.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-03-11
Filing Date
2017-09-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the transportation industry, the existing coating replacement technology is difficult to meet the adhesion and removal requirements of the surface of the vehicle to high wind resistance and composite material surfaces. There are defects in conventional polymer film formation methods such as gelation and lamination defects, which affect the aesthetics. and functional characteristics.

Method used

Using in-situ polymerization of defect-free colored polymer film as the carrier layer, combined with the adhesive layer and the top coating, a multi-layer coating decal is formed, which improves processing efficiency and characteristics, enhances adhesion and recovery, and reduces residual adhesion Mixtures and defects.

Benefits of technology

It achieves better surface covering and removal performance in the transportation industry, reduces defects and weight, improves the durability and aesthetics of coating decals, and is suitable for composite surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909561A_ABST
    Figure CN118909561A_ABST
Patent Text Reader

Abstract

The in-situ polymerized polymer film helps to improve coating film decal, making it have reduced defects. The coated decal includes an in situ polymerized polymer film as a support layer. The carrier layer is colored and preferably defect-free.
Need to check novelty before this filing date? Find Prior Art

Description

Divisional Application Statement

[0001] This application is a divisional application of the PCT international application with international application number PCT / US2017 / 021982 filed on March 11, 2017, and the Chinese invention patent application with invention name “Coated decals, products and methods with reduced defects” and application number 201780057146.1, which entered the Chinese national phase on March 15, 2019. Background Art

[0002] The present invention generally relates to paint film appliques having reduced defects, methods of making and using the same, and articles including the same.

[0003] Painted surfaces are commonly used in many different types of applications. Painted surfaces can not only improve the aesthetic properties of the surface, but they can also improve the functional properties of the underlying surface and help protect them. One such application is in the transportation industry, where the exterior painted surface is typically exposed to a variety of environments, some of which may be very harsh on the surface. Examples of articles with such painted surfaces in the transportation industry include vehicles that provide transportation on land, in water, and in the air. Such vehicles include aircraft and motor vehicles, such as cars and trucks. The coatings on these surfaces can serve to protect the underlying surface from damage caused by such exposure. However, the coating itself must also be durable to withstand repeated exposure to such destructive environments.

[0004] Painting the exterior surfaces of vehicles presents many challenges, not only due to the amount of surface area that typically needs to be painted and the often uneven topography of such surfaces, but also due to increasingly stringent environmental regulations. For example, it is desirable and increasingly regulated to reduce emissions of volatile organic components (VOCs), particularly in industries that utilize large amounts of coatings and other organic chemicals. Thus, VOC reduction and water conservation associated with conventional painting processes are increasingly important environmental considerations.

[0005] A further consideration associated with painting the exterior surfaces of vehicles, particularly in the transportation industry, is the overall weight. The presence of a coating on a surface, while adding to the aesthetic and functional properties of the surface, also adds weight to the article to which it is applied. In the transportation industry, the additional weight results in the consumption of excess fuel and limits the number of passengers or cargo that can be safely and efficiently transported by the associated vehicle.

[0006] Additionally, a unique consideration associated with painting or otherwise covering exterior surfaces on aircraft and similar vehicles is the effect of the relatively high speeds of the vehicle on the vehicle surface and any coating or covering thereon. For example, wind resistance associated with high speed travel may make it difficult to maintain uniform and adequate adhesion of such coatings or coverings to the vehicle surface. As a result, coatings and coverings developed for application to exterior surfaces of moving vehicles (e.g., vehicles traveling on land-based highways) are generally not adequate to withstand the challenging conditions associated with higher travel speeds in the air or on land-based runways.

[0007] In order to overcome the many challenges associated with painting the exterior surfaces of vehicles using traditional methods, many coating replacement technologies have been developed so that the use of traditional coatings can be minimized or avoided. For example, there is a commercially available product that enables automobile manufacturers to completely remove the painting process from the automobile production line by injecting plastic with pigment. This product is sold by Saudi Basic Industries Corporation (SABIC) under the trade name LEXAN SLX, which includes a resin for forming a surface that is traditionally to be painted.

[0008] Other alternatives to using conventional paint include bonding paint replacement films or paint replacement sheets (also known as decals) to surfaces already formed on vehicles. For example, 3M Co., St. Paul, MN, sells paint replacement films and tapes for certain such applications. One such film, 3M TM Paint Replacement Film F577 - described as a polyvinyl chloride film that provides a black textured matte appearance and is used in vehicle window frames, sashes, window extensions, body and door pillars, instrument panel components and covers (metal or plastic). Another such film - 3M TM Paint Replacement Film FTA9055J - Described as being used to provide a blackout look around automotive side glass. This film is described as providing a high gloss (90% reflectivity) black look and an exterior clear coat that can be integrated into the design of a vehicle. See also U.S. Patent Publication No. 2007 / 0047099; U.S. Patent No. 5,965,256; U.S. Patent No. 6,475,616; and U.S. Patent No. 7,141,303, all of which are assigned to 3M Innovative Properties Company.

[0009] Other coating replacement technologies are also known. For example, U.S. Pat. No. 5,034,275 relates to a sheet material coated with a coating. The material is said to include a flexible and stretchable thermoplastic polyester carrier film, a stretchable waterborne polyurethane coating layer, a stretchable transparent cross-linked polyurethane topcoat layer, and a thin tie layer disposed between the carrier film and the coating layer, the tie layer being formed by coating an aqueous dispersion of a neutral copolymer of ethylene and ethylenically unsaturated carboxylic acid on the carrier film.

[0010] U.S. Patent No. 5,114,789 describes a decorative sheet material having a transparent topcoat that can be bonded to a variety of substrates (e.g., automotive exterior panels) as a protective and decorative coating. The sheet material includes a thin carrier film, a coating layer bonded to one surface of the carrier film, and a cross-linked topcoat. In the embodiments described therein, the topcoat is described as "extremely thick" - at least 0.1 mm (100 microns).

[0011] US Patent No. 5,242,751 describes a coating composite article comprising a heat-deformable carrier film having an adhesive layer on a first major surface thereof and a coating layer on a second major surface thereof, the coating layer consisting of a pigmented basecoat covered by a polyurethane topcoat.

[0012] U.S. Patent No. 5,268,215 describes a coating film that is said to have good scratch resistance. A polyurethane coating layer is coated on a polymer carrier film. A polyurethane clearcoat is coated on the upper surface of the coating layer, and then a polyurethane-siloxane topcoat is coated on the clearcoat. The film is said to be capable of being thermoformed, stretched, and adhesively bonded to body parts, boats, household appliances, and other substrates as a protective and decorative covering with a basecoat-clearcoat appearance.

[0013] US Patent No. 5,468,532 describes a multilayer graphic article with a color layer. It is based on a polymer film covered with a protective surface layer, which is said to make the article resistant to weathering and chemical exposure. In an exemplary embodiment, the protective surface layer is described as a polyurethane-based material.

[0014] U.S. Patent No. 6,132,864 describes a painted plastic film coated with two or more layers of specific material coatings. It consists of a base plastic film, which is first coated with a filler composition, then coated with a coloring paint, and then coated with a transparent plastic film. The base plastic film can be a mixture of polyolefins, polyamides, polyurethanes, polyesters, polyacrylates, polycarbonates or different polymer substances. The filler composition is described as a composition containing a binder and a crosslinking agent and other ingredients. The coloring paint coating is described as a topcoat including a polymer binder, with or without a crosslinking agent and a pigment or a pigment mixture. The transparent plastic film is described as being suitable for use as one of the same materials of the base film. It is said that the multilayer sheet described herein has good stone chip resistance and corrosion resistance.

[0015] Despite the availability of a variety of coating replacement technologies, conventional technologies have not satisfactorily addressed coating replacement issues in all cases, particularly with respect to applications involving vehicles used for transportation. Not only is there the problem of adequate adhesion and durability to the exterior surfaces of these vehicles due to the high wind resistance to which these vehicles are typically exposed, but there are other problems as well.

[0016] As an example, many vehicles increasingly rely on composite materials for surfaces bonded with conventional paint substitutes. However, conventional paint substitutes do not typically bond to composite materials as they do to individual materials. It is well known that conventional paint substitutes are not capable of adequately bonding to all surfaces (including surfaces formed by composite materials) and providing the desired aesthetic and functional properties. It is desirable not only that the material be adequately bonded to the surface, but also that the material be easily removed when needed. For example, in the case of aircraft, company logos and designs change frequently, which results in the need to refurbish aircraft that display outdated logos and designs. This is particularly common in the case of leased aircraft, which often undergo multiple and repeated changes in ownership, and thus result in changes in the associated personal or company logos and designs. Typically, when refurbishing the surface, the paint substitute film present on the surface must first be removed. However, many conventional films are not easy to remove because the layers therein are prone to delamination. When the paint substitute film is removed from the surface, the delamination of the paint substitute film significantly complicates the renovation process.

[0017] Even when paint rather than a paint replacement film is present on the surface to be renovated, the renovation process can be problematic. Renovating a painted surface typically requires sanding the surface in preparation for applying a new coat of paint thereon. Composite surfaces typically must rely on sanding to remove unwanted paint thereon when renovating because most chemical strippers cannot be used on composite materials. However, sanding surfaces formed from composite materials is also undesirable because such sanding will likely cause damage (e.g., cracking) to the composite material's reinforcement materials (particularly when the reinforcement materials include fibers).

[0018] As another example, because the preparation methods commonly used to form base films / carrier films conventionally used for multilayer film products (e.g., paint replacement decals) generally involve extrusion and other methods for forming films from compositions that have been polymerized, the chemical and physical properties of these films are limited. U.S. Patent No. 8,828,303 describes some of these limitations. For example, some polymer chemistries cannot be hot melt processed due to their relatively high molecular weight and / or the presence of crosslinking, both of which make hot melt processing of preformed pellets of the composition (usually performed according to conventional methods of forming polymer films using hot melt processing) difficult, if not impossible, to perform at temperatures below the degradation temperature of the polymer composition or substrate on which the film is formed.

[0019] Wet casting polymer film formation methods also have their disadvantages. Whether the system is solvent-based or aqueous, it must first be applied to the desired substrate and then dried to remove the solvation or dispersion medium (i.e., organic solvent or water, respectively) to form a polymer film. Therefore, the use of wet casting methods to form a polymer film of sufficient thickness may be problematic. In addition, due to the lack of sufficient solubility of some polymers or their components in conventional solvents and dispersion media, these polymer chemicals cannot be formed into polymer films using wet casting methods.

[0020] Thus, the properties of conventionally manufactured polymer films are limited to those specific polymer chemistries that can be formed into films using conventional methods, which again typically involve extrusion and other methods for forming films from polymerized compositions. Conventionally manufactured polymer films often have defects caused by at least one of gelation, die lines, and gauge lines due to the methods by which they are formed and the methods by which they are laminated to adjacent films. The prevalence of defects necessitates exhaustive testing and analysis of formed polymer films to ensure that the polymer films are suitable for the intended application due to the negative impact of the defects on, for example, the visual properties of the final product.

[0021] Gelation results in the presence of gel particles (also referred to as "gel") in the final product. "Gel" is generally understood to be a viscous composition, which in polymer processing can be, for example, an at least partially polymerized composition, a composition with a relatively high molecular weight, and / or a composition containing a large amount of entrained gas (e.g., air or reaction byproducts, such as carbon dioxide). Gels can manifest in various forms and are generally caused by overheating during the processing of the polymeric composition into a polymer film. For example, gels can take the form of crosslinks, which are caused by catalyst or other organic or inorganic residues in stagnant and / or dead zones of the resin during extrusion, by degradation-related oxidation occurrences (e.g., carbon dioxide bubbles generated by moisture), or from the supply chain. Gelation can make it difficult to form a uniform layer of polymer material (e.g., a film).

[0022] In addition to forming a polymer film, in order to provide a desired appearance of color or aesthetics for use as a film-coated decal, more than one polymer film (at least one of which is colored) is typically provided and laminated together. However, when the polymer films are laminated together, defects often occur due to the manner in which the polymer films are laminated. Conventionally, polymer films are typically laminated together using heat. However, heat lamination is known to produce a variety of defects. U.S. Patent No. 5,641,374 describes problems associated with defects caused by heat lamination. Those defects include, for example, wrinkles, ripples, curling, excessive shrinkage or stretching, waves, waffles, color density loss, and microbubbles.

[0023] Regardless of their source, defects can cause aesthetic flaws, weak spots and cracks in polymer films and coated appliques and generally compromise their suitability for many applications. Therefore, a great deal of effort is made throughout the supply chain to determine the presence and extent of defects. Many defects can be easily detected when viewed with the naked eye. Other methods of detecting defects, including spectroscopy, can also be used. When defects are detected, the polymer film containing the defects must often be scrapped, resulting in considerable waste.

[0024] As described above, conventional coating replacement technologies fail to adequately address many issues. Therefore, there is still a need for alternative coating replacement technologies. Summary of the invention

[0025] There is a need for alternative polymer films and methods of forming the same for use in related painted decals and articles to impart improved properties thereto. According to the present invention, a colored, in-situ polymerized polymer film is advantageous for improving painted decals. Preferred are defect-free colored polymer films, and painted decals of which the defect-free polymer film is a part, which therefore also have reduced defects.

[0026] In one embodiment, the film-coated decal includes a defect-free colored polymer film as a carrier layer. Compared to conventional multilayer sheets including a conventionally formed polyurethane carrier layer (i.e., such conventional formation generally involves extrusion and other processes for forming a film from an already polymerized composition, wherein polymerization of the material used to form the film is substantially completed prior to forming the film therefrom), the film-coated decal of the present invention does not rely on such a layer as a carrier layer, resulting in improved one or more desired properties in addition to the processing efficiencies imparted thereby.

[0027] Defect-free, colored polymer films used as carrier layers in the film-coated appliques of the present invention are generally described in co-pending PCT Patent Application No. PCT / US17 / 21982, entitled "Defect-Free Polymer Films and Related Protective Sheets, Articles, and Methods," which is incorporated herein by reference in its entirety. Although protective sheets containing ingredients that affect their color and / or transparency are mentioned therein, it is described therein as preferably having a smooth and glossy surface and an overall substantially uniform thickness to maximize their ability to provide seemingly invisible protection to a surface. However, in accordance with the present invention, the polymer films formed according to the disclosure therein are colored for use in film-coated appliques including the polymer films.

[0028] It is understood that, as used herein, when a polymerizable composition is polymerized "in situ" into a desired polymer film, polymerization of the polymer comprising the film begins just before, simultaneously with, or shortly after the polymerizable composition is positioned into the desired film form, and polymerization is substantially complete during or shortly after such positioning. Generally, "just before" and "shortly after" as used to refer to the time when polymerization begins refer to a period of time not exceeding about 30 seconds. Surprisingly, it has been discovered that the use of a colored, in situ polymerized carrier layer helps improve the desired properties of the coated film applique in addition to the processing efficiencies imparted thereby. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a plot of the loss factor (also known as Tan delta) versus temperature for an in-situ polymerized polyurethane carrier layer (which may be colored for use in the film-coated appliques of the present invention) compared to those properties associated with a conventionally formed polyurethane carrier layer.

[0030] Figure 2 is a plot of the storage modulus versus temperature for an in-situ polymerized polyurethane carrier layer (which may be colored for use in the film-coated appliques of the present invention) compared to those properties associated with a conventionally formed polyurethane carrier layer. DETAILED DESCRIPTION

[0031] The phrase "coated decal" encompasses films that include substantially one uniform color throughout, as well as films that, by themselves or in combination with other paint replacement films, include graphics, patterns, and other non-uniformly dispersed color variations throughout. The coated decals of the present invention generally include a colored, in-situ polymerized polymer layer. Although other color layers may be present, the benefits are maximized by using a colored in-situ polymerized polymer layer as a carrier layer in the coated decal. In a further embodiment, the coated decal includes an adhesive layer. The colored in-situ polymerized polymer layer includes at least one color-inducing component and provides a substantially uniform or non-uniform color throughout the coated decal. When the color-inducing component is a pigment, the colored in-situ polymerized polymer layer is also referred to as a "colored layer" in the description of exemplary embodiments of the present invention.

[0032] The coating decals of the present invention advantageously are capable of not only covering a surface, imparting improved properties to the surface, but are also capable of being removed more cleanly than conventional coating decals that include a conventionally formed carrier layer. It has been discovered that by providing a preferably defect-free colored polymer film as a carrier layer (which is capable of absorbing more energy during stretching and / or impact than a conventionally formed carrier layer), adhesive residue remaining on the surface when the coating decal is removed from the surface after use is minimized or eliminated. That is, the improved carrier layer used in the coating decals of the present invention can exhibit more effective damping characteristics (as evidenced by the "peak loss factor" described herein) than conventionally formed carrier layers. Providing such a layer adjacent to other layers in the coating decal helps to form a better continuous bond between the carrier layer and the other layers during application of the coating decal, thereby reducing the likelihood of delamination between the layers and leaving less adhesive and other materials on the surface after the coating decal is removed from the surface.

[0033] According to another aspect of the invention, when such a carrier layer is used according to the invention, the properties of the various layers within the paint film decal are better balanced. For example, when a relatively high modulus topcoat is present in the paint film decal, as in a multi-stage paint (e.g., having the appearance of a conventional basecoat / clearcoat paint finish), a carrier layer having a relatively high loss factor adjacent to such topcoat helps to have a more uniform rate and degree of recovery across the thickness of the paint film decal when the paint film decal is stretched and / or impacted.

[0034] Although the presence of a topcoat is optional, it can be present, for example, in a multistage coating according to the invention comprising a carrier layer (or carrier layers, if desired) in combination with any other color layers, which combination is adjoined on one side by at least one binder layer (i.e. the combination of the aforementioned layers is similar to a basecoat in conventional coating systems) and on the other side by at least one topcoat (i.e. similar to a clearcoat in conventional coating systems).

[0035] It should be understood that the number of levels of a multi-stage coating generally corresponds to the number of topcoats within the coating applique. For example, in one embodiment of a two-stage coating according to the present invention, the coating applique consists essentially of the following layers: an adhesive layer, a carrier layer, and a topcoat. In another embodiment of a two-stage coating according to the present invention, the coating applique consists essentially of the following layers: an adhesive layer, a carrier layer, a different color layer, and a topcoat, wherein the carrier layer and the different color layer are positioned between the adhesive layer and the topcoat in any order. An exemplary three-stage coating according to the present invention may include any of the foregoing two-stage coatings, any of which has an additional topcoat adjacent to the first topcoat.

[0036] Preferably, the coating decals of the present invention are advantageously capable of not only covering surfaces with better balanced properties and leaving less residual adhesive after removal from the surface, but they also have enhanced recoverability to enable them to adequately cover and be easily applied to non-planar surfaces. As used herein, "recoverability" refers to the ability of a material to be stretched and substantially return to its original state after stretching. The preferred coating decal is capable of substantially returning to its original state when stretched (i.e., elongated) to a length of up to about 125% of its original length. Preferably, the coating decal is capable of substantially returning to its original state when stretched to a length of up to about 150% of its original length. According to one aspect of the present invention, the coating decal is capable of being elongated to a length of up to greater than about 200% of its original length before breaking.

[0037] According to an exemplary embodiment of the present invention, due to its formation method, the painted decal advantageously includes a defect-free colored polymer film as a carrier layer. In a further embodiment, the painted decal having a defect-free colored polymer film as a carrier layer also includes at least one of a topcoat layer and an adhesive layer.

[0038] According to one aspect of this further embodiment, the coating applique comprises the following sequential layers: a defect-free colored polymer film as a carrier layer; an optional color layer; and an adhesive layer. According to another aspect of this further embodiment, the coating applique comprises the following sequential layers: an optional color layer; a defect-free colored polymer film as a carrier layer; and an adhesive layer. According to yet another aspect of this further embodiment, the coating applique comprises the following sequential layers: a topcoat layer; a defect-free colored polymer film as a carrier layer; and an optional color layer. According to yet another aspect of this further embodiment, the coating applique comprises the following sequential layers: a topcoat layer; an optional color layer; and a defect-free colored polymer film as a carrier layer.

[0039] Further embodiments of the latter two aspects include an adhesive layer in sequence such that the adhesive layer is exposed outwardly adjacent to the optional color layer or carrier layer. An exemplary film-coated decal comprises the following sequential layers: a topcoat layer; a defect-free colored polymer film as a carrier layer; an optional color layer; and an adhesive layer. Another exemplary film-coated decal comprises the following sequential layers: a topcoat layer; an optional color layer; a defect-free colored polymer film as a carrier layer; and an adhesive layer.

[0040] For ease of handling and to minimize weight and cost, the total thickness of the film-coated decal is preferably less than about 130 microns. In one embodiment, the total thickness of the film-coated decal is from about 100 microns to about 130 microns. In another embodiment, the total thickness of the film-coated decal is from about 50 microns to about 75 microns. Each individual and discrete layer within the film-coated decal is described in further detail below.

[0041] Carrier layer

[0042] By using "carrier layer" herein, it is understood that the polymer film comprising it carries (i.e., supports) at least one other layer (e.g., an optional adhesive layer, an optional color layer, or an optional topcoat) in the film-coated applique. Although the thickness of the other layers, either individually or collectively, may be greater than the thickness of the carrier layer, the carrier layer is a necessary element to provide the film-coated applique with the desired properties, whether those properties are aesthetic, functional, or otherwise.

[0043] When assembling the coating decal of the present invention, the carrier layer is polymerized in situ on the adjacent layers. According to a preferred embodiment of the present invention, a defect-free colored layer (the colored layer is one or more) of a polymer film supporting at least one other layer is used as a carrier layer. In some cases, the carrier layer may also be referred to as a "base layer", "support layer" or similar names. Generally, the carrier layer of the coating decal of the present invention is called a "mid-ply layer" when it contains multiple layers (i.e., "n" individual layers). However, according to other embodiments of the present invention, the carrier layer of the coating decal of the present invention may be a single film layer. When multiple layers form the carrier layer, each of the "n" individual layers may have the same or different chemical compositions. In an exemplary embodiment, each of the "n" individual layers has substantially the same chemical composition.

[0044] The carrier layer is colored, but another different color layer may be provided depending on the application. For example, a color layer may be provided between the carrier layer and the adhesive layer. Alternatively, or in combination with another color layer, a color layer may be provided on the outer surface of the carrier layer. In this embodiment, the carrier layer may be impregnated with a material (e.g., titanium dioxide) that causes the carrier layer to act as a reflective background, showing the color of the overlying color layer when the film decal is applied to the surface.

[0045] According to a preferred aspect of the present invention, the carrier layer used in the film-coated applique of the present invention is polyurethane-based. For simplicity, the term "polyurethane" as used herein includes polymers containing urethane (also known as carbamate) bonds, urea bonds or combinations thereof (i.e., in the case of poly(urethane-urea)). Thus, the polyurethane-based carrier layer contains at least urethane bonds, urea bonds or combinations thereof. Furthermore, the polyurethane-based carrier layer is based on a polymer wherein the polymer backbone has at least 40%, preferably at least 60%, and more preferably at least 80% urethane and / or urea repeating bonds formed in situ during the polymerization process.

[0046] The polyurethane-based carrier layer is prepared by reacting the components according to the method of the present invention, the components including at least one isocyanate-reactive (e.g., hydroxyl-functional, such as polyol) component and at least one isocyanate-functional (e.g., polyisocyanate) component. For example, the components of an exemplary polymerizable composition for forming a polyurethane-based carrier layer according to the method of the present invention are described in U.S. Pat. No. 8,828,303, entitled "Methods for Polymerizing Films In-Situ Using a Radiation Source", which is incorporated herein by reference in its entirety. In a preferred embodiment, the polymerizable composition according to this aspect of the present invention includes an aliphatic component, more preferably substantially consisting of an aliphatic component.

[0047] In an exemplary embodiment, at least one radiation source selected from ultraviolet radiation, thermal radiation, and electron beam radiation is used to initiate polymerization of the polymerizable composition. The method of the present invention can be used in a continuous process or a batch process. For example, in one embodiment of the present invention, a continuous process can be used, such as using relatively low energy ultraviolet radiation (e.g., having less than about 100 mW / cm 2 The in-situ polymerization of the polyurethane-based carrier layer can be performed based on the web. As another example, in another embodiment of the present invention, batch processing can be used, such as coating a UV-curable composition onto a discrete substrate and irradiating it to form a polyurethane-based carrier layer in situ.

[0048] According to a preferred aspect of the inventive method, the polymerizable composition for forming the carrier layer is substantially free of solvent. However, unlike hot melt systems that may be substantially free of solvent, the polymerizable composition according to the preferred aspects of the present invention is liquid when applied to a substrate (the composition will be polymerized on the substrate) at room temperature. In addition to environmental and safety issues such as those associated with solvent-based processing, solvent-based processing generally requires the use of elevated temperatures for effectively removing excess solvent from the polymerized composition. Therefore, preferably, the carrier layer is substantially free of unreacted solvent. Therefore, preferably, the polymerizable composition forming them is substantially free of solvent. According to these preferred embodiments, sustainable coating technology is promoted.

[0049] The carrier layer comprises at least one color-inducing component. In its broadest sense, color-inducing components include those components that affect only the opacity of the carrier layer, those components that affect only the spectral color of the carrier layer, and those components that affect only the tint, shade or tone of the carrier layer. In the case of those components that affect opacity, an opaque carrier layer and therefore an opaque coating decal can be obtained. In the case of a component that affects hue, shade or tone, it is understood that hue is the mixture of a color with white, which increases brightness. Chroma is the mixture of a color with black, which reduces brightness. Hue is produced by mixing a color with gray, or by hue and chroma together. Mixing a color with any neutral color (including black, gray and white) reduces chroma or colorfulness, while hue remains unchanged.

[0050] Color-inducing ingredients useful in the present invention include, for example, those substances commonly referred to as pigments, coatings, colorants, metal flakes, and dyes by those of ordinary skill in the art. Pigments are an exemplary color-inducing ingredient. In an exemplary embodiment, the color layer includes ink. Any suitable commercially available ink can be used. Non-limiting examples of suitable inks include pigmented acrylic inks (including pigmented quick-drying acrylic inks), pigmented polyurethane inks, epoxy inks, and polyurethane enamel coatings, such as those sold under the trade name DESOTHANE HS by PRC Desoto International, Inc. of Glendale, CA.

[0051] When the carrier layer is colored, it is surprisingly found that the amount of pigment required to impart the same color to the carrier layer (of the present invention) is lower than the amount of pigment required to add to conventionally form a polymer film used as a carrier layer. Therefore, according to the present invention, any adverse effects on the ductility or other properties of the carrier layer due to the addition of pigment are minimized. According to one aspect of the present invention, it will be understood by those of ordinary skill in the art that the resulting carrier layer is elastic in nature. In order to obtain these benefits in a polyurethane-based polymer film or other similar polymer film polymerized from a plurality of reactive components, preferably, a color-inducing component is added to at least two of the plurality of components that are mixed and reacted. This provides benefits in terms of processing efficiency.

[0052] In addition to the color inducing component, any suitable additives can be present in the carrier layer. Other additives known to those skilled in the art are selected based on the intended application. Those skilled in the art can easily determine the amount of these additives to obtain the desired effect.

[0053] According to one embodiment of the present invention, the thickness of the carrier layer is from about 5 microns to about 1250 microns. According to a further embodiment, the thickness of the carrier layer is from about 8 microns to about 260 microns. Where each of the "n" individual film layers can be as thin as about 5 microns and up to about 50 microns thick, the presence of thicker layers is particularly useful, for example, in ballistic applications. However, in order to impart greater recoverability, according to one aspect of the present invention, a carrier layer having a thickness of about 220 microns or less is used. According to a further aspect, the thickness of the carrier layer is about 180 microns or less. For example, the thickness of the carrier layer may be from about 120 microns to about 180 microns. By using a thinner carrier layer, not only is the recoverability of the carrier layer, and therefore the recoverability of the entire film-coated decal, enhanced, but the overall cost of the film-coated decal is reduced in this manner.

[0054] Compared to conventional film-coated decals that include a conventionally formed carrier layer (i.e., such conventional formation generally involves extrusion and other methods of forming a film from an already polymerized composition, wherein polymerization of the material used to form the film is substantially complete prior to forming the film therefrom), the film-coated decals of the present invention do not rely on such a layer as a carrier layer, resulting in unexpected improvements in one or more desired properties in addition to the processing efficiencies thereby imparted. For example, problems associated with dimensional instability of extruded films (such as those described in U.S. Pat. No. 5,985,079) can be minimized.

[0055] According to one aspect of the present invention, the improved polyurethane-based carrier layer in the film-coated decal of the present invention is in-situ polymerized. For example, U.S. Patent No. 8,828,303 and U.S. Patent Application Publication No. US-2011-0137006-A1, both of which are incorporated herein by reference, describe films and methods formed by such in-situ polymerization. Surprisingly, we have found that using an in-situ polymerized carrier layer to impart color to a film-coated decal helps improve desired physical properties in addition to the processing efficiency thereby imparted.

[0056] Unlike conventional carrier layers, which are typically extruded, the in-situ polymerized carrier layers of the present invention are generally not thermoplastic in nature. However, the look and feel of the in-situ polymerized carrier layers of the present invention are very similar to conventional extruded carrier layers. However, the improved polymer structure provides the in-situ polymerized carrier layers of the present invention with some significantly different properties, including dimensional stability.

[0057] Another significantly different property is solvent resistance. The solvent resistance of the preferred in-situ polymerized support layer of the present invention approaches that of conventional cross-linked (i.e., thermosetting) materials. As is often the case with thermoplastic materials, extruded materials will generally dissolve completely when immersed in a solvent (e.g., tetrahydrofuran), whereas the in-situ polymerized material of the present invention exhibits only slight swelling when immersed in the same solvent.

[0058] Another significantly different property is the storage modulus. As is common with thermoplastic materials, extruded materials typically exhibit a continuous decrease in storage modulus with increasing temperature. However, the storage modulus of the preferred in-situ polymerized carrier layer of the present invention is significantly different: it exhibits a rubbery plateau region, a feature consistent with a lightly crosslinked elastomer. In one embodiment, the storage modulus of the preferred in-situ polymerized polyurethane-based carrier layer is about two orders of magnitude higher than the storage modulus of thermoplastic polyurethane at conventional extrusion temperatures.

[0059] According to another aspect of the invention, the improved polyurethane-based carrier layer in the film-coated applique of the present invention has a peak loss factor of at least about 0.5, at least about 0.8, or even at least about 1.2 when tested as a stand-alone film according to the Loss Factor Test Method described below.

[0060] like Figure 1As shown, the peak loss factor of the extruded (i.e., conventionally formed) polyurethane carrier layer film tested according to the Loss Factor Test Method described below (i.e., as shown by the data curves labeled A, B, and C, which represent extruded polyurethane-based carrier layers available from Argotec, LLC (Greenfield, MA) under the trade names ARGOTEC 49510, ARGOTEC 49510-60DV, and ARGOTEC 46510, respectively) is significantly lower than that of the carrier layer film to which the color-inducing component may be added according to the present invention, which has a peak loss factor greater than 0.5 (i.e., as shown by the data curves labeled 1 and 2). As also shown Figure 1 As shown, the peak loss factor of the extruded polyurethane carrier film test occurs at about 25°C, while the peak loss factor of the polyurethane base film used in combination with the color-inducing component used as a carrier layer in the coating applique of the present invention occurs at a temperature of about at least 35°C.

[0061] In addition, for the tested polyurethane-based films used as a carrier layer in combination with the color-inducing component in the coated film applique of the present invention, the half-height loss factor (which is half of the peak loss factor value, two for each curve) appears in a temperature range below about 40°C, in some embodiments below about 30°C, and even in some embodiments below about 20°C, whereas for the extruded polyurethane-based polymer film, in exemplary embodiments, the half-height loss factor appears in a temperature range above about 40°C, even above about 45°C. Figure 1 The data curves marked as A and B in the figure show that the half-height loss factor is 53°C. Figure 1 The data curve marked as C in the figure shows that the half-height loss factor is 49°C. Figure 1 The half-height loss factor is 18°C. Figure 1 In the data curve marked as 2, the half-height loss factor was measured to be 22°C.

[0062] like Figure 2 As shown, the storage modulus of the extruded (i.e., conventionally formed) polyurethane film tested according to the storage modulus test method described below (i.e., as shown by the data curves labeled A, B, and C) is reduced to a specific value at a relatively lower temperature than the storage modulus of the polyurethane-based polymer film used as the carrier layer in combination with the color-inducing component in the coating applique of the present invention.

[0063] As described above, preferably, the carrier layer in the coated film applique of the present invention is not only colored, but also defect-free. As used herein, "defects" should be understood as visual defects, such as gel particles, die lines, or gauge lines. As used herein, "defect-free" refers to a polymer film having no more than the maximum allowable defects shown in Table 1, as described by the maximum defect diameter.

[0064] Table 1 Preferably, there are no detectable defects in the polymer film when viewed by the naked eye. More preferably, there are no detectable defects in the polymer film when viewed at a magnification of up to about 50 times.

[0065] Advantageously, in preferred embodiments, because the polymer film used as a carrier layer is not formed in a conventional reactor, a conventional p-gel is not formed. Likewise, in preferred embodiments, because a conventional extruder is not used to form the polymer film, a conventional e-gel is not formed. Once polymerized, the preferred polymer film used as a carrier layer in the coated decal of the present invention has never undergone thermoplastic deformation, has never been through an extruder, and has never undergone thermal extrusion at conventional extrusion temperatures. In addition, given that the preferred polymer film is not formed using a conventional extruder, when assembling the coated decal according to the present invention, processing aids - such as lubricating and anti-blocking additives - which are known to assist in gel formation and are conventionally required and used in such formation methods are not required, and are preferably excluded, from the method of forming the polymer film. The resulting polymer film is defect-free and colored, and the coated decal incorporating the polymer film as a part thereof has reduced defects.

[0066] Optional color layer

[0067] Although at least one color layer different from the defect-free colored polymer film can be used in further embodiments of the coated decal of the present invention, for simplicity, we will refer to one such optional color layer for description below. It should be recognized that if multiple color layers are used, each color layer can be the same or different.

[0068] When a color layer is present, the color layer comprises any suitable material and provides the desired aesthetic effect when the film decal is applied to a surface. The color layer can be a continuous or discontinuous layer. Note that the color layer can consist essentially of a graphic, pattern, etc., which makes the layer a discontinuous layer and / or a non-planar layer.

[0069] The color layer includes at least one color-inducing component. In its broadest sense, color-inducing components include those components that affect only the opacity of the color layer, those components that affect only the spectral color of the color layer, and those components that affect only the hue, chroma or tone of the color layer. In the case of those components that affect opacity, an opaque color layer and, therefore, an opaque coating decal can be obtained. In the case of components that affect hue, chroma or tone, it is understood that hue is the mixture of a color with white, which increases brightness. Chroma is the mixture of a color with black, which reduces brightness. Hue is produced by mixing a color with gray, or by hue and chroma together. Mixing a color with any neutral color (including black, gray and white) reduces the chroma or chroma, while the hue remains unchanged.

[0070] Color-inducing components useful in the present invention include, for example, those substances commonly referred to as pigments, coatings, colorants, metal flakes, and dyes by those of ordinary skill in the art. Pigments are an exemplary color-inducing component. In an exemplary embodiment, the color layer includes ink. Any suitable commercially available ink may be used. Non-limiting examples of suitable inks include pigmented acrylic inks (including pigmented quick-drying acrylic inks), pigmented polyurethane inks, epoxy inks, and polyurethane enamel coatings, such as those sold under the trade name DESOTHANE HS by PRC Desoto International, Inc. of Glendale, CA.

[0071] Any suitable additives may optionally be included in the color layer. For example, stabilizers (e.g., antioxidants, heat stabilizers, and UV stabilizers), crosslinkers (e.g., aluminum or melamine crosslinkers), corrosion inhibitors, plasticizers, photocrosslinkers, additional colorants, fillers, and other conventional additives known to those skilled in the art may be incorporated into the color layer.

[0072] Preferably, if a color layer is present, the color layer is substantially free of constituents that may tend to migrate to the outer surface of the film-coated applique or interfaces therein, where such constituents may promote delamination between the layers or otherwise adversely affect the adhesion of the film-coated applique to an adjacent surface or layer. The color layer is also preferably resistant to chemicals to which it may be exposed during use of the film-coated applique. For example, it is preferred that the color layer resist degradation by water and hydraulic fluids (e.g., those sold under the trade name Solutia, Inc.'s SKYDROL by TBM, Inc. of St. Louis, MO), particularly when the color layer comprises an outer layer of the film-coated applique after the film-coated applique is applied to a surface.

[0073] The color layer can be formed according to any suitable method. In one embodiment, the color layer is formed by solution casting of the polymerized composition. For example, the color layer can be formed by solution casting of an organic solvent. As another example, the color layer can be cast by an aqueous solution.

[0074] In yet another embodiment, the color layer is in situ polymerized. As described above, U.S. Patent No. 8,828,303 and U.S. Patent Publication No. US-2011-0137006-A1 describe films and methods formed by such in situ polymerization. A preferred aspect of this embodiment is that the color layer is network polymerized from a solvent-free polymerizable composition that is a liquid in neat form at room temperature.

[0075] In a preferred embodiment, the color layer is a reactive polymer film. "Reactive" is understood to mean that the polymer film includes chemical functions so that the carrier layer polymerized thereon can form covalent bonds with the color layer at the interface between two adjacent layers (i.e., the carrier layer and the color layer). According to one aspect of this embodiment, the reactive polymer film includes hydroxyl functional groups that are capable of reacting with, for example, isocyanate functional groups in the polymerizable composition forming the carrier layer.

[0076] When a color layer is present, the color layer comprises any suitable thickness. According to one embodiment of the present invention, the thickness of the color layer is from about 5 microns to about 1250 microns. According to a further embodiment, the thickness of the color layer is from about 8 microns to about 260 microns. In another further embodiment, the thickness of the color layer is from about 12 microns to about 125 microns. In another further embodiment, the thickness of the color layer is from about 25 microns to about 75 microns. In yet another further embodiment, the thickness of the color layer is from about 8 microns to about 25 microns. For example, as long as the color of the film decal is fully visible outward when the film decal is applied to the surface, the thickness of the color layer can vary significantly without departing from the spirit and scope of the present invention. While enhancing the flexibility of the entire film decal by using a thinner color layer, the overall cost of the film decal can also be reduced in this way.

[0077] Optional adhesive layer

[0078] When there is adhesive layer, adhesive layer is adjacent to and is positioned at a principal plane side of carrier layer and any optional other color layer, relative to the principal plane side of any optional topcoat layer thereon.Any suitable adhesive can be used for adhesive layer according to the present invention.In a preferred embodiment, adhesive layer comprises pressure sensitive adhesive.

[0079] Although any suitable chemical substance can be used for the base polymer in the adhesive layer, (meth)acrylates, i.e., acrylate and methacrylate chemicals, are preferred. However, other suitable chemicals are known to those skilled in the art, including, for example, chemicals based on synthetic and natural rubber, polybutadiene and its copolymers, polyisoprene and its copolymers, and siloxanes (e.g., polydimethylsiloxane and polymethylphenylsiloxane). Any suitable additive can be present in combination with the base polymer in the adhesive layer.

[0080] In particular, adhesives based on the polymerization of 2-ethylhexyl acrylate, vinyl acetate and acrylic acid monomers as known to those skilled in the art find use in one embodiment of the invention. The adhesive may be crosslinked, for example, using conventional aluminum or melamine crosslinking agents.

[0081] In one embodiment, the thickness of adhesive layer is about 5 microns to about 150 microns. In a further embodiment, the thickness of adhesive layer is about 10 microns to about 100 microns. In another further embodiment, the thickness of adhesive layer is about 30 microns to about 100 microns. However, without departing from the spirit and scope of the present invention, the thickness of adhesive layer can significantly change.

[0082] Before the adhesive layer is applied to a surface, a conventional release liner, for example, may be used to protect the adhesive layer. In this way, the sheet can be easily stored and transported in a roll or other form until its application.

[0083] Optional topcoat

[0084] Generally, a topcoat refers to any outwardly exposed non-adhesive layer on the major planar side of a carrier layer and any optional color layer (when present) (the color layer and carrier layer are laminated together), the topcoat being opposite to any adhesive layer in the film-coated applique of the present invention. Consistent with its name, the topcoat that is optionally present is the outer layer of the film-coated applique that is exposed outwardly when the film-coated applique is applied to an article. Any suitable type of material can be used for the topcoat in the film-coated applique of the present invention. For example, the topcoat can include polycarbonate, polyvinyl fluoride, poly(meth)acrylate (e.g., polyacrylate or polymethacrylate), polyurethane, its modified (e.g., hybrid) polymer, or a combination thereof as a base polymer. See U.S. Patent No. 4,476,293, which describes an exemplary polycarbonate-based polyurethane for the topcoat of the present invention. See also U.S. Patent Publication No. US-2008-0286576-A1, which is incorporated herein by reference, for further exemplary topcoats.

[0085] In one embodiment, a topcoat is applied (e.g., by spraying or painting) to the film-coated decal after it is bonded to the underlying surface. Preferably, in this embodiment, the topcoat is applied so that none of the film-coated decal is exposed to the environment when the decal is bonded to the surface for use. Further, when more than one film-coated decal is used in combination with others on a surface, the topcoat preferably covers and protects the seams between adjacent film-coated decals from exposure to the environment.

[0086] In another embodiment, the topcoat is one of the layers included in the coating decal. For example, the multi-stage coating according to the present invention includes a carrier layer (or multiple carrier layers, if necessary), optionally combined with at least one color layer, one side of the color layer is at least one adhesive layer (i.e., the aforementioned layers are combined similar to the base coat in the traditional coating system), and the other side is at least one topcoat (i.e., similar to the clear coat in the traditional coating system). The two-stage coating according to this exemplary embodiment has 1 topcoat. The three-stage coating according to this exemplary embodiment has two adjacent but different topcoats.

[0087] The topcoat may include any suitable chemical. Typically, the topcoat provides one or more properties including the following: environmental resistance, chemical resistance, abrasion resistance, scratch resistance, optical clarity, and other generally desired properties. When the film-coated decal is applied to the article, the carrier layer or the color layer, either of which would be exposed to the outside in any other manner, may provide the desired properties so that a topcoat is no longer required, but particularly, the presence of a topcoat is beneficial when this is not the case. According to an exemplary embodiment, the topcoat includes a material having the following properties: no yellowing, gloss retention (e.g., maintaining gloss at a level of about 80 to about 90 gloss units), and ductility.

[0088] In an exemplary embodiment, the topcoat comprises a polyurethane-based material. Many suitable topcoats are commercially available, including, for example, polyurethane coatings sold under the trade name DESOTHANE HS by PRC Desoto International, Inc. of Glendale, CA (e.g., DESOTHANE HS BAC 900 (CA8000 / B900A or CA8000 / B900B)) or polyurethane coatings sold under the trade name ECLIPSE by Akzo-Nobel Aerospace Coatings of Waukegan, IL (e.g., ECLIPSE BAC 900).

[0089] Preferably, the chemical composition of the topcoat is selected to promote its bonding to the underlying layer of the film-coated decal. According to one aspect of this embodiment, the surface tension of the underlying layer of the film-coated decal is within about 5 dynes / cm of the surface tension of the overlying topcoat. According to another aspect of this embodiment, the topcoat includes an excess of isocyanate functional moieties that react with excess isocyanate reactive moieties in the underlying layer of the film-coated decal to which the topcoat is applied. According to this aspect of the invention, covalent bonds are formed between the topcoat and the underlying layer of the film-coated decal. Such covalent bonds are generally stronger than other types of bonds (e.g., bonds that rely on van der Waals forces, such as those typically formed using pressure sensitive adhesives) and are therefore preferred.

[0090] Preferably, in order to maximize the gloss retention, antifouling and other desired performance characteristics of the film decal, the topcoat has a relatively high molecular weight. That is, while the topcoat can be formed by extrusion according to some embodiments of the present invention, the topcoat preferably has a sufficient molecular weight that makes its extrusion impractical (i.e., if it is a polyurethane, one of ordinary skill in the art would not consider the polyurethane to be an extrusion grade polyurethane). In a preferred embodiment, in addition to the carrier layer of the present invention, the topcoat is also polymerized in situ.

[0091] In one embodiment, when the topcoat is present, the thickness of the topcoat is from about 1 micron to about 28 microns. In a further embodiment, the thickness of the topcoat is from about 5 microns to about 20 microns. In another further embodiment, the thickness of the topcoat is from about 5 microns to about 15 microns. In another further embodiment, the thickness of the topcoat is from about 5 microns to about 12 microns. In another further embodiment, the thickness of the topcoat is from about 5 microns to about 7 microns. However, without departing from the spirit and scope of the present invention, the thickness of the topcoat can vary significantly.

[0092] To protect the topcoat (when present), a polymer liner (eg, a clear polyester liner) or the like may be used and removed either before or after the film-coated decal is applied to the substrate.

[0093] Formation of coating decals

[0094] Each individual layer of the film decal is formed and assembled into a multi-layer film decal according to the knowledge of those skilled in the art. However, when forming the carrier layer, the carrier layer is formed in situ on the adjacent layers, which may include the optional different color layers, optional adhesive layers and / or optional topcoats of the film decal.

[0095] To prepare the adhesive layer, any suitable method may be used. For example, as an alternative to forming the adhesive layer directly (e.g., in situ) on the carrier layer, according to one embodiment and as known to those skilled in the art, an adhesive film of a desired thickness may be cast onto a release film. In this embodiment, the adhesive film supported on the release film may then be assembled with the carrier layer, wherein the release film is removed prior to bonding the film-coated decal to the surface of the article.

[0096] Although there are no other limitations in terms of method and assembly order, at least the carrier layer is polymerized in situ. According to a further aspect of this embodiment, each other individual layer of the film-coated decal is prepared before being assembled into the film-coated decal. As known to those skilled in the art, any suitable method for forming each other individual layer can be used.

[0097] In order to prepare the optional topcoat, any suitable method can be used. For example, according to one embodiment and as known to those skilled in the art, a film including a topcoat with a desired thickness can be cast onto a smooth film (e.g., polyester film) to form a supported topcoat. In one embodiment, the supported topcoat is then assembled onto a carrier layer or onto the outwardly exposed side of a laminate including a carrier layer and an optional color layer (when it exists), i.e., assembled onto the main surface relative to the main surface with which any optional adhesive layer is assembled. The smooth film used to form the topcoat can be retained in the assembly until the film decal is applied to the article surface to provide additional protection during transportation and storage of the sheet. According to this embodiment, any suitable method can be used to assemble the topcoat with the remaining layer of the film decal. According to another embodiment, the topcoat is formed according to a conventional method by applying the topcoat directly onto the remaining layer of the film decal.

[0098] While the above method requires forming separate layers and then bonding these layers together to form a film-coated decal, according to another embodiment of the present invention, some layers of the film-coated decal can be formed simultaneously, for example, by coextruding the polymerizable composition starting in liquid form of the polymerizable composition, which step is generally carried out at a temperature below about 40°C - for example, in one embodiment at about room temperature. In addition to the carrier layer, the layers other than the carrier layer can also be polymerized in situ into a film form, which film form is described in, for example, U.S. Patent No. 8,828,303 and U.S. Patent Publication No. US-2011-0137006-A1. Regardless of the method used, the process can be a continuous process or a batch process.

[0099] Application of coating decals

[0100] The film-coated decals of the present invention are used in a range of indoor and outdoor applications in, for example, the transportation, construction and sporting goods industries. The film-coated decals can be advantageously applied to at least a portion of the surface of any article requiring a coating. These articles include, for example, motor vehicles (e.g., automobiles and airplanes) and non-motor vehicles (e.g., conventional bicycles) and many other applications. The surface to which the film-coated decal is applied can be painted or unpainted.

[0101] Although the paint decals of the present invention may have a textured outwardly exposed surface when applied to an underlying substrate, it is preferred that the paint decals of the present invention have a smooth surface and a substantially uniform thickness throughout to maximize their ability to provide desired aesthetic properties to a surface.

[0102] During use, the film-coated decal is preferably applied to the surface in a manner that conforms to the shape of the surface. Recoverability is important and preferred, especially when the film-coated decal is applied to non-planar surfaces. If the film-coated decal does not recover well, microcracks will occur when the decal is pulled too far. In this case, a relief cut may be required to apply such a film-coated decal to a substrate, especially a substrate with a complex surface having convex and concave features. However, according to a preferred embodiment of the present invention, when the film-coated decal of the present invention is applied to a complex surface, a relief cut is not required. Such a film-coated decal is easily adaptable due to its recoverability.

[0103] Based on the knowledge of those skilled in the art, the film-coated decals of the present invention can be applied to the surface of the article without difficulty and easily. The adhesive layer (if present) is usually bonded to the surface to which the film-coated decal is applied after removing any release liner present thereon to expose the adhesive. When a pressure-sensitive adhesive layer is used, the film-coated decal can be more easily repositioned before being firmly bonded to the surface. Example Exemplary Test Methods

[0104] Exemplary embodiments and applications of the present invention are described in conjunction with the following test methods.

[0105] Loss Factor Test Method

[0106] The test was conducted in tension mode using a dynamic mechanical analyzer purchased from TA Instruments (New Castle, DE) under the trade name TA Instruments DMA Q800. Nominal sample dimensions of 5-12 mm in length, 4-8 mm in width, and 0.02-0.2 mm in thickness were used. Values ​​for determining the loss factor of the samples were measured using a frequency of 1 Hz, a strain of 0.3%, and a heating rate of 3°C / min.

[0107] Storage modulus test method

[0108] The test was conducted in tension mode using a dynamic mechanical analyzer available from TA Instruments (New Castle, DE) under the trade name TA Instruments DMA Q800. Nominal sample dimensions of 5-12 mm in length, 4-8 mm in width, and 0.02-0.2 mm in thickness were used. Values ​​for determining the storage modulus of the samples were measured using a frequency of 1 Hz, a strain of 0.3%, and a heating rate of 3°C / min.

[0109] Solvent resistance test method

[0110] Small discs (25 mm diameter x 0.16 mm thickness) of each material were immersed in separate jars, each containing 16 mL of tetrahydrofuran (THF). The dissolution and / or swelling of the discs of each example was evaluated after 5 minutes. To evaluate each sample, if the disc was no longer intact, the contents of the jar were poured into a 200 mesh stainless steel filter. If no solid or gel residue was trapped on the screen, it was confirmed that the disc material had completely dissolved and was not simply broken into fine fragments. If the disc was still intact at 5 minutes, the disc was kept immersed in THF for a total of 6 hours. After a total of 6 hours of immersion, the disc was still there, and the disc was removed from the jar and its diameter was immediately measured. Thereafter, the disc was allowed to air dry. After approximately twenty-four hours, the diameter of the disc was measured again.

[0111] Comparative Example C1

[0112] ARGOTEC 49510 thermoplastic polyurethane film discs available from Argotec, LLC (Greenfield, MA) were evaluated according to the Solvent Resistance Test Method described above. After five minutes, the disc was no longer intact and was confirmed to be completely dissolved.

[0113] Comparative Example C2

[0114] ARGOTEC 46510 thermoplastic polyurethane film discs available from Argotec, LLC (Greenfield, MA) were evaluated according to the Solvent Resistance Test Method described above. After five minutes, the disc was no longer intact and was confirmed to be completely dissolved.

[0115] Example 1

[0116] Discs of film 3 prepared according to the following exemplary formulation (see Tables 2 and 5) were evaluated according to the above solvent resistance test method. After 6 hours of soaking, the diameter of the disc was measured to be 160% of its original size. After air drying, the disc returned to its original 25 mm diameter, confirming the evaporation of THF. Exemplary formulations

[0117] Defect-free polymer films and coated film appliques including the same can be prepared according to the method described in US Pat. No. 8,828,303 and using the following ingredients for each layer.

[0118] Element

[0119] Table 2

[0120] Carrier layer

[0121] Three different carrier layers for the coated film appliques of the present invention were formed based on the ingredients described in Table 2 and the proportional amounts shown in Tables 3 to 5. The weight percentages are reported based on the total weight of the resulting film including the carrier layer.

[0122] Table 3 (film 1) weight% Element 47.72871 High molecular weight polyols 26.11440 Medium molecular weight polyol A 0.47007 Low molecular weight polyols 0.00441 catalyst 0.88668 UV Initiator 0.44334 UV Stabilizers 9.85239 Isocyanate 14.50000 Masterbatch

[0123] Table 4 (film 2)

[0124] Table 5 (film 3) weight% Element 9.53127 Medium molecular weight polyol B 20.25396 Medium molecular weight polyol D 9.43596 Low molecular weight polyols 0.00441 catalyst 0.88668 UV Initiator 0.44334 UV Stabilizers 49.44438 Isocyanate 10.00000 Masterbatch

[0125] Top coating

[0126] The acrylic-based polyurethane topcoat used in the film-coated applique of the present invention is formed from aliphatic acrylic polyols and aliphatic polyisocyanate polymers which are polymerized in situ on the carrier layer after being coated to a thickness of about 10 microns.

[0127] Adhesive layer

[0128] The adhesive layer used for the coating applique of the present invention is formed based on the adhesive composition described in Table 2 and is located on the carrier layer opposite to the top coating layer.

[0129] Various modifications and variations of the present invention will be apparent to those skilled in the art without departing from the spirit and scope defined by the appended claims of the present invention. It should be noted that the steps listed in any of the following method claims do not necessarily need to be performed in the order in which they are listed. One of ordinary skill in the art will understand the changes in steps made from the order in which they are listed.

[0130] Any theory presented herein is subject to modification pending further testing and analysis. Thus, the inventors do not intend to be bound by any theory presented herein, such as what factors contribute to the described physical properties of the film-coated applique and the various layers therein combined.

Claims

1. A coating decal, comprising: Optionally, a topcoat; a carrier layer comprising at least one color-inducing component; Optionally, different color layers; as well as Optionally, an adhesive layer; wherein the storage modulus of the carrier layer exhibits a rubbery plateau as the temperature increases; and wherein the carrier layer has: (a) a peak loss factor of at least 0.5; (b) a peak loss factor occurring at a temperature of at least 35°C; and / or (c) a half-height loss factor of the carrier layer occurring in a temperature range below 40°C; all of these loss factors when tested as a stand-alone film according to the Loss Factor Test Method.

2. The coating decal according to claim 1, characterized in that: The film-coated decals are opaque.

3. The coating decal according to claim 1, characterized in that: The carrier layer provides a substantially uniform or non-uniform color across the entire film-coated decal.

4. The coating decal according to claim 1, characterized in that: The carrier layer is defect-free.

5. The coating decal according to claim 1, characterized in that: The carrier layer and / or the topcoat layer are polyurethane-based.

6. The coating decal according to claim 1, characterized in that: The support layer does not contain unreacted solvent.

7. The coating decal according to claim 1, characterized in that: The coating decal comprises the top coating layer, the carrier layer, the different color layer and the adhesive layer in sequence.

8. The coating decal according to any one of claims 1 to 6, characterized in that: The coating decal comprises the top coating layer, the different color layer, the carrier layer and the adhesive layer in sequence.

9. The coating decal according to any one of claims 1 to 6, characterized in that: The coating decal comprises the top coating layer, the carrier layer and the adhesive layer in sequence.

10. The coating decal according to claim 1, characterized in that: The film-coated decal includes the adhesive layer, and the adhesive layer includes a pressure-sensitive adhesive.

11. The coating decal according to claim 1, characterized in that: The film-coated decal includes the adhesive layer and further includes a release film located on an outer surface of the adhesive layer.

12. The coating decal according to claim 1, characterized in that: The thickness of the coating decal is less than 130 microns.

13. The coating decal according to claim 1, characterized in that: The coating decal includes the top coating layer, and the top coating layer has a thickness of 5 micrometers to 20 micrometers.

14. A coating decal formed according to any one of the preceding claims, characterized in that: The method comprises: forming the carrier layer; Optionally, forming the topcoat layer; Optionally, forming the different color layers; and Optionally, the adhesive layer is formed.

15. The method according to claim 14, characterized in that The method includes polymerizing the support layer in situ.

16. The method according to claim 14, characterized in that The carrier layer includes a pigment.

17. The method according to claim 14, characterized in that The method includes forming the support layer on a reactive film, the reactive film including the different color layer adjacent to the support layer.

18. The method according to claim 14, characterized in that The different color layer is present, and the method includes forming the different color layer by in situ polymerization, and includes forming the support layer and the different color layer by coextrusion of a polymerizable composition, the polymerizable composition being polymerized in situ to simultaneously form the support layer and the different color layer.

19. The method according to claim 14, characterized in that The method also includes forming the topcoat layer.

20. The method according to claim 14, characterized in that The different color layers are solution cast.

21. The method according to claim 14, characterized in that The method includes casting the different color layers from an organic solvent solution.

22. The method according to claim 14, characterized in that The method includes casting the different color layers from an aqueous solution.

23. The method according to claim 14, characterized in that The support layer includes the reaction product of reactants including an aliphatic polyisocyanate and three polyols.

24. The method according to claim 23, characterized in that One of the polyols has a number average molecular weight of 1400 to 2000, and one of the polyols comprises a polyether polyol.

25. The method according to claim 23, characterized in that One of the polyols has a number average molecular weight of 900 to 1400, and one of the polyols comprises a polyether polyol.

26. The method according to claim 14, characterized in that The method includes forming the support layer from a substantially solvent-free polymerizable composition.

27. The method according to claim 14, characterized in that The support is formed using ultraviolet radiation and / or electron beam radiation.

28. A method of coating the surface of a substrate, the method comprising applying a coating decal according to any one of claims 1 to 13 to the surface.