Acid and alkali resistant heat sealing adhesive for PTP and PTP cover film

By using heat sealing glue made of hydroxyacrylic resin and polyvinylidene chloride-polyester-rubber composite materials, the barrier problem of PTP aluminum foil packaging on acidic and alkaline drugs is solved, and the heat sealing strength and shelf life are improved. It is suitable for Polypropylene blister packaging, especially when liquid medicines are heat sealed, maintaining high strength to avoid deterioration and leakage of drugs.

CN118909569APending Publication Date: 2024-11-08JIANGYIN BAOBO PACKING +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411026289.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When faced with acidic or alkaline drugs, existing PTP aluminum foil packaging cannot effectively block the migration of substances, resulting in premature failure of the drug's shelf life, especially poor heat sealing of liquid drugs, which poses a risk of deterioration or leakage of drugs.

Method used

Using hydroxyacrylic resin, polyvinylidene chloride-polyester-rubber composite materials as heat sealant, combined with epoxy silane coupling agent and slippery agent, high-performance heat sealant is made by blending it through a twin-screw extruder. , and form a multi-layer film in the polypropylene blister packaging to enhance barrier, mechanical strength and flexibility.

Benefits of technology

It realizes effective packaging of acidic and alkaline drugs, improves heat seal strength and shelf life, especially in the case of small heat seal area, avoids deterioration and leakage of drugs, and meets the high-performance heat seal of polypropylene blisters need.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909569A_ABST
    Figure CN118909569A_ABST
Patent Text Reader

Abstract

The invention discloses an acid-resistant and alkali-resistant heat-sealing adhesive for PTP (polytrimethylene terephthalate) and a PTP cover film. Comprising the following raw materials in parts by weight: 20-40% of hydroxy acrylic resin, 50-70% of a polyvinylidene chloride-polyester-rubber polymer, 3-5% of an epoxy silane coupling agent and 2-5% of a slipping agent. The acid and alkali resistant heat-sealing adhesive for PTP can be used for packaging acid and alkali drugs at the same time; the applicability is wide, and heat sealing with a polypropylene bubble cap is completely met; particularly, when a liquid medicine is subjected to heat sealing, and the heat sealing contact area of the bubble cap and the bottom film is small, the heat sealing can still keep high strength, and the problem that the packaging quality guarantee period is too early and fails due to poor heat sealing is solved. Due to the fact that the heat sealing adhesive contains an acrylic acid system and the addition of the ethylene propylene diene monomer rubber, the heat sealing layer can have good binding force with non-polar materials such as PP and PE, and the acid and alkali resistance is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging materials, and in particular to an acid-resistant and alkali-resistant heat-sealing adhesive for PTP and a PTP cover film. Background Art

[0002] PTP aluminum foil is a special material used for drug packaging in the pharmaceutical industry. Its full name is "Press-Through Packaging" aluminum foil, or commonly known as "blister aluminum foil". PTP aluminum foil is mainly used for blister packaging, which is a way to seal products (such as tablets, capsules, etc.) between plastic blisters and aluminum foil to protect the products from air, humidity and light, while providing convenient single-dose dispensing.

[0003] PTP aluminum foil provides excellent oxygen, moisture and light barrier, extending the shelf life of medicines. It also has good tearability, making it easy for consumers to take out medicines. It also has good processing properties.

[0004] Most of the existing blister packaging materials are PVC sheets, and the covering materials of blister packaging are basically aluminum foil. However, due to the presence of chlorine in PVC, this material will cause certain pollution to the environment when it is treated as solid waste after use.

[0005] Polypropylene materials are gradually being used in the market due to the absence of chlorine elements. However, due to the non-polarity of polypropylene materials, if the existing VC agent is still used, the heat sealing strength of polypropylene materials is insufficient.

[0006] In addition, some contents contain free acidic or alkaline substances. The existing conventional PTP aluminum foil cannot effectively block the migration and volatilization of acidic and alkaline substances, resulting in the problem of premature expiration of the shelf life of the packaging.

[0007] For example, oral iodic acid anti-inflammatory tablets in current medicines and povidone-iodine liquid in medical devices will decompose acidic substances to corrode the aluminum foil layer during long-term storage, leading to serious problems such as reduction of the effective ingredients in the contents and corrosion and cracking of the aluminum foil.

[0008] In order to achieve the acid-blocking effect, Chinese Patent 200510038218.7 discloses a primer with acid-blocking function, which uses copolymers of ethylene glycol-terephthalic acid-sebaic acid as the main adhesive resin, and is matched with a mixed resin of nitrocellulose, acrylic resin, ethylene glycol-terephthalate-isoprene glycol copolymer and a mixed organic solvent to form a solvent-based glue. The film generated after coating has the high density and insoluble properties of thermosetting resin, and has the higher surface tension of thermoplastic resin, that is, efficient secondary coating can be carried out on the film generated.

[0009] Chinese patent 201710060776.6 discloses a method for preparing an acid-barrier aluminum foil cover film for blister packaging and a cover film, which adopts two steps: 1. respectively preparing an adhesive layer mixture, a barrier coating mixture and a heat-sealing layer mixture; 2. coating the adhesive layer mixture, performing a first heating treatment, coating the barrier coating mixture, performing a second heating treatment, coating the heat-sealing layer mixture and performing a first drying treatment to obtain a blister packaging sheet product; the barrier coating adopts hydroxyl acrylic resin and polyvinylidene chloride as matrix resins, and the two resins are rapidly cured under the action of a cross-linking agent and a catalyst, and are cross-linked and rearranged to form a functional film layer with good acid resistance and barrier properties, thereby preventing the migration of small molecular acidic substances and HCl, and ensuring that the effective ingredients of the blister contents are not reduced.

[0010] However, the existing heat-sealing glue cannot fully meet the requirements of PP heat sealing, nor is it resistant to acid and alkaline liquid medicines. It reacts with medicines, especially liquid medicines, and causes the medicines to deteriorate or leak. Especially when heat-sealing liquid medicines, when the heat-sealing area with the bottom film is small, there will be problems of poor heat sealing, or the shelf life of the packaging will expire prematurely.

[0011] In view of the above, it is necessary to propose an acid-resistant and alkali-resistant heat-sealing adhesive and a PTP cover film for PTP to solve the above problems. Summary of the invention

[0012] The purpose of the present invention is to overcome the defects in the prior art and provide an acid-resistant and alkali-resistant heat-sealing adhesive and a PTP cover film for PTP.

[0013] To achieve the above object, the technical scheme of the present invention is as follows: an acid-resistant and alkali-resistant heat-sealing adhesive for PTP, comprising the following raw materials in parts by weight: 20-40% of hydroxy acrylic resin, 50-70% of polyvinylidene chloride-polyester-rubber polymer, 3-5% of epoxy silane coupling agent, and 2-5% of lubricant; The polymer of polyvinylidene chloride-polyester-rubber is made by blending polyvinylidene chloride (PVDC), polyester and rubber; the polyvinylidene chloride is 25-40%, polyester is 20-40%, and rubber is 10-15%. PVDC is a chlorine-containing polymer, which is known for its excellent gas and water vapor barrier properties. Therefore, it is more suitable for food packaging films and other applications that require high barrier properties. Polyester is a large class of polymers, the most common of which is polyethylene terephthalate. In the present invention, the polyester uses polyethylene terephthalate (PET). PET is widely used in the fields of textiles, beverage bottles, engineering plastics and films.

[0014] Furthermore, the rubber is one or more of ethylene propylene diene monomer rubber (EPDM), styrene butadiene rubber (SBR), and nitrile butadiene rubber (NBR). They have good elasticity, wear resistance, and chemical resistance, and are widely used in tires, seals, shock-absorbing components, etc. In the present invention, PVDC can be used to form a barrier, polyester provides mechanical strength and formability, and rubber may increase flexibility or improve impact resistance. Such a composite material can have a good acid and alkali resistance effect when facing the encapsulation of acid and alkaline drugs, can provide better comprehensive performance, and in the encapsulation process of the blister cover film, a high-performance multilayer film is formed, which has good barrier and acid and alkali resistance effects.

[0015] Specifically, in the present invention, hydroxy acrylic resin is used as an adhesive and can effectively enhance flexibility; polyvinylidene chloride (PVDC) is used to provide barrier properties and improve the barrier properties of the heat sealing layer; polyester uses polyethylene terephthalate (PET) as a filler and is used to provide strength and thermal stability to improve the temperature resistance of the heat sealing adhesive; and rubber plays a role in increasing flexibility, so that the formed heat sealing layer has good flexibility.

[0016] Furthermore, the compatibility between PVDC, polyester and rubber is limited, so a compatibilizer is required. The silane coupling agent acts as a compatibilizer to promote fusion, specifically 3-aminopropyltrimethoxysilane (KH-550) or 3-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560).

[0017] Furthermore, the lubricant is a type of additive used to improve the processing performance of polymers and the performance of final products. They mainly reduce the internal friction of the polymer melt and the external friction between the melt and the processing equipment, thereby making the material smoother during processing, reducing the adhesion between products, and improving production efficiency and product quality; specifically, one or more of oleamide, erucamide, zinc stearate, and calcium stearate, and combined with their compatibility with the polymer matrix to improve specific performance, processing conditions and other factors.

[0018] A method for preparing an acid-resistant and alkali-resistant heat-sealing adhesive for PTP is intended to create a composite material having acid-resistant and alkali-resistant properties, high temperature resistance, and good flexibility, and to improve barrier properties, mechanical strength, and flexibility. Specifically, the method comprises the following steps: S1, raw material preparation, preparing granules or powders of hydroxy acrylic resin, PVDC, polyester and rubber, and other additives and auxiliaries; S2, blending and compounding, using a twin-screw extruder or internal mixer to blend the components in S1, controlling the processing temperature and time to ensure that the polymers are fully melted and evenly mixed, and adding compatibilizers to improve the compatibility between different polymers; setting the temperature of the twin-screw extruder at 220~280℃ to ensure that the hydroxylated acrylic resin, PVDC, and polyester are fully melted without degradation; each polymer has its own specific processing temperature window, which needs to be carefully controlled to avoid degradation caused by overheating S3, granulation, the blended melt is formed into small particles through a water-cooled granulation system, and these particles serve as the basic material of the heat-sealing adhesive; S4, preparing a film or coating layer, remelting the particles in step S3 and forming a film through a casting or blow molding process; or, coating the molten colloid on a substrate using a coating device; S5, cooling and curing, cooling the adhesive film or adhesive layer by means of a cooling roller or an air knife to solidify it.

[0019] S6, heat seal test, heat seal test is carried out under different temperature, pH and pressure conditions to evaluate the performance of heat seal adhesive.

[0020] A PTP cover film comprises a heat sealing layer, a barrier layer and a printing layer, wherein the heat sealing layer comprises a film layer or a coating layer made of the aforementioned heat sealing adhesive, the barrier layer and the printing layer constitute an aluminum foil cover film, and a film layer is arranged between a polypropylene blister and the barrier layer; or, a coating layer is formed by coating the polypropylene blister and the printing layer on both or either side.

[0021] The advantages and beneficial effects of the present invention are as follows: the acid- and alkali-resistant heat-sealing adhesive for PTP of the present invention can be used for the packaging of acidic and alkaline drugs at the same time; it has wide applicability and fully meets the requirements of heat-sealing with polypropylene blisters; especially when heat-sealing liquid drugs, when the heat-sealing contact area between the blister and the bottom film is small, the heat-sealing can still maintain a high strength, and the problem of premature failure of the package shelf life due to poor heat-sealing will not occur. Since the heat-sealing adhesive contains an acrylic acid system, the addition of EPDM rubber can make the heat-sealing layer have a good bonding force with non-polar materials such as PP and PE, and has good acid and alkali resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a structural schematic diagram of a PTP cover film of the present invention; In the figure: 1. Polypropylene blister; 2. Heat seal layer; 3. Barrier layer; 4. Printing layer; 5. Aluminum foil cover film. DETAILED DESCRIPTION

[0023] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.

[0024] Embodiment 1: Hydroxylated acrylic resin: 20%; PVDC: 40%; PET: 30%; EPDM: 10%; Compatibilizer: 5%; Lubricant: 5%; Processing steps: 1. Use a twin-screw extruder for melt blending.

[0025] 2. Control the temperature of the extruder between 220°C and 250°C to ensure that PVDC and PET are fully melted without degradation.

[0026] 3. Add compatibilizer to promote the compatibility between different polymers.

[0027] 4. Cooling and granulation.

[0028] 5. A multilayer film is formed by co-extrusion technology, in which the PVDC layer is used as a barrier layer, PET is used as a support layer, and hydroxylated acrylic resin and EPDM are used as heat-sealing layers.

[0029] Embodiment 2: Hydroxylated acrylic resin: 35%; PVDC: 25%; PET: 20%; EPDM: 15%; Silane coupling agent: 3%; Lubricant: 3%; Antioxidants and heat stabilizers: 2%; Processing steps: 1. Use a high-speed mixer to mix the dry powder evenly.

[0030] 2. The mixture was fed into a twin-screw extruder for melt blending.

[0031] 3. Control the processing temperature between 250°C and 280°C to ensure that the material does not undergo thermal degradation.

[0032] 4. Make heat sealant granules through granulator.

[0033] 5. Test the high temperature stability and bonding performance of heat sealant.

[0034] Embodiment three: Hydroxylated acrylic resin: 25%; PVDC: 35%; PET-G (modified PET): 30% (improves transparency and impact resistance); SBR: 10%; Silane coupling agent: 5%; Lubricant: 5%; Processing steps: 1. Use a twin-screw extruder for melt blending.

[0035] 2. Control the extruder temperature between 230°C and 260°C to ensure that the material is melted and the transparency is not affected.

[0036] 3. Form a transparent composite film through a casting process.

[0037] 4. Cool, coil and test for clarity and barrier properties.

[0038] Performance Test: A PTP cover film, such as Figure 1 As shown, it includes a heat sealing layer 2, a barrier layer 3, and a printing layer 4. The heat sealing layer 2 includes a film layer or a coating layer made of the aforementioned heat sealing adhesive. The barrier layer 3 and the printing layer 4 constitute an aluminum foil cover film 5. A film layer is provided between the polypropylene blister 1 and the barrier layer 3; or, a coating layer is formed by coating the polypropylene blister 1 and the printing layer 4 on both or either side. The thickness of the heat sealing layer 2 is 2 to 6 microns. The heat sealing adhesive prepared by the method is used to coat the printing layer 4, which overcomes the problem that the existing heat sealing adhesive is not acid-resistant and alkali-resistant and is easy to leak, and the softness is significantly improved; the printing layer 4 is 40 to 60 g / m 2 , heat sealant coating amount 10g / m 2 , cut into 2.5*10cm, fit the printed layer 4 coated with heat seal glue to the cover of the polypropylene blister 1, and heat-press seal them with a common heat sealer, and then perform solvent barrier test, water vapor permeability test, and oxygen permeability test on the PTP cover film made in each embodiment; the solvent barrier test includes placing an acid solution and an alkaline solution in the polypropylene blister 1 to determine the barrier performance of the heat seal layer 2 to a specific solvent; the water vapor permeability test adopts a weighing method: the permeability is calculated by measuring the change in mass of water vapor before and after passing through the sample within a certain period of time; the oxygen permeability test adopts a pressure difference method: a pressure difference is established on both sides of the film to measure the flow rate of oxygen.

[0039] Solvent barrier test Water vapor transmission rate test Oxygen Transmission Rate Test Embodiment 1 Not disclosed Flux is 0g / (m²·day) Flux is 0cm³ / (m²·day·atm) Embodiment 2 Not disclosed Flux is 0g / (m²·day) Flux is 0cm³ / (m²·day·atm) Embodiment 3 Not disclosed Flux is 0g / (m²·day) Flux is 0cm³ / (m²·day·atm) The heat-sealing adhesive of the present invention has wide applicability and fully meets the requirements for heat-sealing with polypropylene blisters; especially when heat-sealing liquid medicines, when the heat-sealing contact area between the blister and the bottom film is small, the heat-sealing can still maintain a high strength, and the problem of premature failure of the package shelf life due to poor heat sealing will not occur. Since the heat-sealing adhesive contains an acrylic acid system, the addition of EPDM rubber can make the heat-sealing layer have a good bonding force with non-polar materials such as PP and PE, and has good acid and alkali resistance.

[0040] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A kind of acid and alkali resistant heat sealing adhesive for PTP, It is characterized in that The invention is prepared by the following raw materials in parts by weight: 20-40% of hydroxy acrylic resin, 50-70% of polyvinylidene chloride-polyester-rubber polymer, 3-5% of epoxy silane coupling agent, and 2-5% of lubricant; The polyvinylidene chloride-polyester-rubber polymer is prepared by blending polyvinylidene chloride (PVDC), polyester and rubber; the polyvinylidene chloride is 25-40%, the polyester is 20-40% and the rubber is 10-15%.

2. The acid-resistant and alkali-resistant heat-sealing adhesive for PTP according to claim 1, It is characterized in that The polyester is polyethylene terephthalate (PET).

3. The acid-resistant and alkali-resistant heat-sealing adhesive for PTP according to claim 1, It is characterized in that The rubber is one or more of ethylene propylene diene monomer rubber (EPDM), styrene butadiene rubber (SBR), and nitrile butadiene rubber (NBR).

4. The acid-resistant and alkali-resistant heat-sealing adhesive for PTP according to claim 1, It is characterized in that The silane coupling agent is 3-aminopropyltrimethoxysilane or 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

5. The acid-resistant and alkali-resistant heat-sealing adhesive for PTP according to claim 1, It is characterized in that The lubricant is one or more of oleamide, erucamide, zinc stearate and calcium stearate.

6. A method for preparing an acid-resistant and alkali-resistant heat-sealing adhesive for PTP according to claim 1, It is characterized in that The following steps are involved: S1, raw material preparation, preparing granules or powders of hydroxy acrylic resin, PVDC, polyester and rubber, and other additives and auxiliaries; S2, blending and compounding, using a twin-screw extruder or an internal mixer to blend the components in S1, controlling the processing temperature and time to ensure that the polymers are fully melted and evenly mixed, and adding a compatibilizer to improve the compatibility between different polymers; S3, granulation, the blended melt is formed into small particles through a water-cooled granulation system, and these particles serve as the basic material of the heat-sealing adhesive; S4, preparing a film or coating layer, remelting the particles in step S3 and forming a film through a casting or blow molding process; or, coating the molten colloid on a substrate using a coating device; S5, cooling and curing, cooling the adhesive film or adhesive layer by a cooling roller or an air knife to solidify it; S6, heat seal test, heat seal test is carried out under different temperature, pH and pressure conditions to evaluate the performance of heat seal adhesive.

7. A method for preparing an acid-resistant and alkali-resistant heat-sealing adhesive for PTP according to claim 6, It is characterized in that In the step S2, the temperature of the twin-screw extruder is set at 220-280° C. to ensure that the hydroxylated acrylic resin, PVDC, and polyester are fully melted without being degraded.

8. A PTP cover film, It is characterized in that The invention comprises a heat sealing layer, a barrier layer and a printing layer, wherein the heat sealing layer comprises a film layer or a coating layer made of the heat sealing adhesive according to claim 1, the barrier layer and the printing layer constitute an aluminum foil cover film, and a film layer is arranged between the polypropylene blister and the barrier layer; or, a coating layer is formed by coating the polypropylene blister and the printing layer on both or either side.