Green bio-based polyurethane adhesive for bamboo winding pipe and preparation method thereof
By preparing green bio-based polyurethane adhesives, environmental pollution and health risks caused by petroleum-based adhesives are solved, and the application of environmentally friendly adhesives is realized, and the environmental protection performance and service life of bamboo-wrapped composite pipes are improved.
Patent Information
- Application Number
- CN202411184724.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The petroleum-based adhesives used in the production of existing bamboo-wrapped composite pipes cause environmental pollution and health risks, and the petroleum resources are limited, so environmentally friendly bio-based adhesives need to be developed to replace traditional adhesives.
Using the preparation method of green bio-based polyurethane adhesive, the bio-based polyurethane prepolymer is generated by reacting raw materials such as aliphatic isocyanate, bio-based polyol, catalyst, chain extender and acetone, and modified with soy protein solution and polyphenol compounds. Nanofiller blends to prepare an environmentally friendly adhesive suitable for bamboo-wrapped composite pipes.
This method not only reduces the consumption of non-renewable resources and reduces carbon emissions, but also enhances the anticorrosion, antibacterial, waterproof and flame retardant properties of adhesives through nanocomposite materials, and improves the environmental protection performance and service life of bamboo-wrapped composite pipes.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane adhesives, and relates to a green bio-based polyurethane adhesive for bamboo-wound pipes. The invention also relates to a preparation method of the green bio-based polyurethane adhesive for bamboo-wound pipes. Background Art
[0002] In recent years, bamboo-wrapped composite materials have garnered widespread attention as a key alternative to traditional plastic products, driven by environmental concerns. During the production of bamboo-wrapped composite pipes, adhesives bond the bamboo layers, enhance structural strength, improve durability, and optimize the production process, ensuring the overall performance and service life of the pipe. Currently, the production of bamboo-wrapped composite pipes primarily relies on petroleum-based adhesives such as urea-formaldehyde resin, phenolic resin, and polyurethane. However, the use of these adhesives poses environmental and health risks, particularly given the limited availability of petroleum resources and the increasing pollution associated with their production. To address these challenges, the development of environmentally friendly adhesives based on renewable bioresources has become essential. Bio-based waterborne polyurethanes, with their excellent biocompatibility, low carbon footprint, and biodegradability, have become a promising candidate for replacing petroleum-based adhesives. By manipulating their soft and hard segment structures, their overall performance can be improved to suit diverse applications. Furthermore, bio-based polyurethanes can effectively enhance the adhesion properties of soy protein adhesives, providing a more environmentally friendly alternative. Therefore, the use of bio-based polyurethane not only meets the requirements of sustainable development, but also can improve the environmental performance of bamboo-wrapped composite pipes, and provide technical support for the application of new bio-based adhesives in this field. Summary of the Invention
[0003] The purpose of the present invention is to provide a method for preparing a green bio-based polyurethane adhesive for bamboo-wound pipes. The adhesive prepared by this method can not only achieve adhesion to the bamboo-wound pipes, but also reduce the consumption of non-renewable resources, thereby achieving the purpose of environmental protection.
[0004] Another object of the present invention is to provide a green bio-based polyurethane adhesive for bamboo-wound pipes.
[0005] The first technical solution adopted by the present invention is a method for preparing a green bio-based polyurethane adhesive for bamboo winding pipes, which specifically includes the following steps:
[0006] Step 1: adding an aliphatic isocyanate, a bio-based polyol, a catalyst, a chain extender, and acetone to a reaction vessel in sequence, introducing nitrogen, and then heating and stirring to obtain a bio-based polyurethane prepolymer;
[0007] Step 2, preparing a bio-based polyurethane emulsion according to the product obtained in step 1;
[0008] Step 3: blending the bio-based polyurethane emulsion obtained in step 2 with a soybean protein solution, a curing agent, and a nanofiller modified with a polyphenol compound, and stirring the mixture evenly at room temperature to obtain a bio-based polyurethane adhesive for bamboo-wrapped composite pipes.
[0009] The first technical solution of the present invention is also characterized in that:
[0010] In step 1, the mass of the aliphatic isocyanate is 10-18 g, the mass of the bio-based polyol is 24-35 g, the mass of the catalyst is 50-100 μL, the mass of the chain extender is 3-10 g, and the volume of acetone is 30 mL.
[0011] In step 1, the aliphatic isocyanate is one of hexamethylene diisocyanate, isophorone diisocyanate and trimethylhexamethylene diisocyanate;
[0012] The bio-based polyol is at least one of a plant oil-based polyol and a wood fiber-based polyol;
[0013] The catalyst is at least one of dibutyltin dilaurate, stannous octoate, stannous oleate, and lead isooctanoate;
[0014] The chain extender is one of dimethylol propionic acid, dimethylol butyric acid, dihydroxy half ester, sodium ethylenediamine sulfonate and diethylenetriamine.
[0015] In step 1, the heating temperature is 75-85° C. and the stirring time is 4-6 h.
[0016] The specific process of step 2 is:
[0017] The temperature of the reaction vessel was lowered to 25-50° C., a salt-forming agent was added to the bio-based polyurethane prepolymer obtained in step 1 and stirred for 0.5-1 h to form a salt, and then 130-180 mL of deionized water was added and stirred for 0.5-1.5 h to emulsify, and finally rotary evaporation was performed at 55° C. to obtain a bio-based waterborne polyurethane emulsion.
[0018] In step 2, the salt-forming agent is one of triethylamine, ammonia water, and sodium hydroxide, and the amount of the salt-forming agent used is 3-7 mL.
[0019] In step 3, the soy protein solution is prepared by dissolving the soy protein in 70-85 mL of deionized water and stirring for 1-2 hours, wherein the mass of the soy protein is 15-30 g.
[0020] In step 3, the preparation process of the polyphenol compound modified nanofiller is as follows:
[0021] The nanofiller is ultrasonically dispersed in deionized water for 15 minutes to obtain a 10 mg / mL nanofiller dispersion, and then the polyphenol compound is dissolved in deionized water to obtain a 1 mg / mL polyphenol compound aqueous solution. Subsequently, the polyphenol compound aqueous solution is added dropwise to the nanofiller dispersion, stirred at room temperature for 2 hours, and centrifuged to obtain a polyphenol compound-modified nanofiller powder; the volume of the nanofiller dispersion is 8-12 mL, and the volume of the polyphenol compound aqueous solution is 0.5-2 mL.
[0022] In step 3, the mass ratio of bio-based polyurethane emulsion: soy protein solution: polyphenol-modified nanofiller: curing agent is 1:0.5-1.5:0.01-0.1:0.02-0.15;
[0023] The curing agent is at least one of dicyandiamide, diaminodiphenylmethane, and diaminodiphenyl sulfone;
[0024] The polyphenol compound is one of tannic acid, gallic acid and polydopamine, and the nanofiller is one of lithium algae, zirconium hydrogen phosphate and layered double hydroxide; and the polyphenol compound modified nanofiller is obtained.
[0025] The second technical solution adopted by the present invention is that the green bio-based polyurethane adhesive for bamboo-wound pipes is prepared by adopting the preparation method of the green bio-based polyurethane adhesive for bamboo-wound pipes.
[0026] The beneficial effects of the present invention are as follows:
[0027] (1) The present invention selects green and safe aliphatic isocyanate and biopolyol as the main raw materials, uses nanocomposite materials for reinforcement, and compounds with soy protein to prepare an environmentally friendly polyurethane adhesive. On the existing basis, it greatly reduces the carbon emissions during the production and use of winding pipes.
[0028] (2) The present invention increases the anti-corrosion, antibacterial, waterproof, flame retardant and other application properties of the adhesive by introducing different nanocomposite fillers, thereby realizing its application in various environments. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to specific embodiments.
[0030] The preparation method of the green bio-based polyurethane adhesive for bamboo winding pipes of the present invention specifically comprises the following steps:
[0031] Step 1: 10-18 g of aliphatic isocyanate, 24-35 g of bio-based polyol, 50-100 μL of catalyst, 3-10 g of chain extender, and 30 mL of acetone are sequentially added to a reaction vessel, nitrogen is introduced, and the mixture is heated and stirred at 75-85° C. for 4-6 hours to obtain a bio-based polyurethane prepolymer;
[0032] wherein the aliphatic isocyanate is one of hexamethylene diisocyanate, isophorone diisocyanate and trimethylhexamethylene diisocyanate;
[0033] The bio-based polyol is one or more of plant oil-based polyol and wood fiber-based polyol;
[0034] The catalyst is one or more of dibutyltin dilaurate, stannous octoate, stannous oleate, and lead isooctanoate;
[0035] The chain extender is one of dimethylol propionic acid, dimethylol butyric acid, dihydroxy half ester, sodium ethylenediamine sulfonate and diethylenetriamine;
[0036] Step 2: Lowering the system temperature in the reaction vessel to 25-50° C., adding a salt-forming agent to the bio-based polyurethane prepolymer and stirring for 0.5-1 hour, then adding 130-180 mL of deionized water and stirring for 0.5-1.5 hours for emulsification, and finally performing rotary evaporation at 55° C. to obtain a bio-based waterborne polyurethane emulsion; the salt-forming agent is one of triethylamine, ammonia water, and sodium hydroxide; and the volume of the salt-forming agent is 3-7 mL;
[0037] Step 3: Add water at room temperature and stir for 1-2 hours to dissolve 15-30 g of soy protein in 70-85 mL of deionized water to obtain a soy protein solution;
[0038] Step 4: blend the bio-based polyurethane emulsion, soy protein solution, polyphenol-modified nanofiller, and curing agent in a mass ratio of 1:0.5-1.5:0.01-0.1:0.02-0.15, and stir evenly at room temperature to obtain a bio-based polyurethane adhesive for bamboo-wrapped composite pipes.
[0039] The preparation process of the polyphenol compound-modified nanofiller is as follows:
[0040] The nanofiller is ultrasonically dispersed in deionized water for 15 minutes to obtain a 10 mg / mL nanofiller dispersion, and then the polyphenol compound is dissolved in deionized water to obtain a 1 mg / mL polyphenol compound aqueous solution. Subsequently, the polyphenol compound aqueous solution is added dropwise to the nanofiller dispersion, stirred at room temperature for 2 hours, and centrifuged to obtain a polyphenol compound-modified nanofiller powder; the volume of the nanofiller dispersion is 8-12 mL, and the volume of the polyphenol compound aqueous solution is 0.5-2 mL.
[0041] The polyphenol compound is one of tannic acid, gallic acid, and polydopamine;
[0042] The nanofiller is one of lithium algae, zirconium hydrogen phosphate, and layered double hydroxide; the polyphenol compound modified nanofiller is obtained, and the specific combination includes one of lithium algae @ tannic acid, zirconium hydrogen phosphate @ gallic acid, and layered double hydroxide @ polydopamine;
[0043] The curing agent is at least one of dicyandiamide, diaminodiphenylmethane and diaminodiphenyl sulfone.
[0044] Example 1
[0045] Step 1: 13 g of isophorone diisocyanate, 24 g of vegetable oil-based polyol, 3.5 g of dihydroxymethylbutyric acid, 50 μL of dibutyltin dilaurate, and 30 mL of acetone were added to a 250 mL three-necked flask, nitrogen was introduced, and the mixture was heated to 75°C for 4 hours. The temperature was then lowered to 40°C, 3 mL of triethylamine was added dropwise, and the reaction was continued for 0.5 hours. Finally, 170 mL of deionized water was added and stirred for 0.5 hours, and the resulting emulsion was then rotary evaporated at 55°C to remove excess acetone to obtain a bio-based polyurethane emulsion with a solid content of approximately 25%.
[0046] Step 2: dissolving 25 g of soy protein in 75 mL of deionized water and stirring for 2 h to obtain a soy protein solution;
[0047] Step 3: Ultrasonic dispersion of zirconium hydrogen phosphate nanosheets in deionized water for 15 minutes to obtain a 10 mg / mL zirconium hydrogen phosphate dispersion; then, gallic acid is dissolved in deionized water to obtain a 1 mg / mL gallic acid aqueous solution, and then the gallic acid aqueous solution is added dropwise to the zirconium hydrogen phosphate dispersion, stirred at room temperature for 2 hours to obtain a zirconium hydrogen phosphate@gallic acid dispersion, and centrifuged and dried to obtain a zirconium hydrogen phosphate@gallic acid nanofiller; the volume of the zirconium hydrogen phosphate dispersion is 8 mL, and the volume of the gallic acid aqueous solution is 0.5 mL.
[0048] Step 4: blend the bio-based polyurethane emulsion, soy protein solution, zirconium hydrogen phosphate@gallic acid nanofiller, and dicyandiamide in a mass ratio of 1:0.5:0.01:0.02, and stir evenly at room temperature to obtain a bio-based polyurethane adhesive for bamboo-wrapped composite pipes.
[0049] Example 2
[0050] Step 1: Add 10g of hexamethylene diisocyanate, 30g of wood fiber-based polyol, 3g of dimethylolbutyric acid, 80μL of dibutyltin dilaurate and 30mL of acetone to a 250mL three-necked flask, introduce nitrogen, and heat to 80°C for 5h. Then cool to 25°C, add 5mL of triethylamine dropwise, and continue to react for 0.8h. Finally, add 130mL of deionized water and stir for 1h, then rotary evaporate the resulting emulsion at 55°C to remove excess acetone to obtain a bio-based polyurethane emulsion with a solid content of approximately 25%;
[0051] Step 2: dissolving 15 g of soy protein in 70 mL of deionized water and stirring for 1 h to obtain a soy protein solution;
[0052] Step 3: ultrasonically disperse the lithium ion nanosheets in deionized water for 15 minutes to obtain a 10 mg / mL lithium ion dispersion; then, dissolve tannic acid in deionized water to obtain a 1 mg / mL tannic acid aqueous solution, and then add the tannic acid aqueous solution dropwise to the lithium ion dispersion, stir at room temperature for 2 hours to obtain a lithium ion @ tannic acid dispersion, and centrifuge and dry to obtain a lithium ion @ tannic acid nanofiller; the volume of the lithium ion dispersion is 10 mL, and the volume of the tannic acid aqueous solution is 1 mL.
[0053] Step 4: blend the bio-based polyurethane emulsion, soy protein solution, lithium algae @ tannic acid nanofiller, and dicyandiamide in a mass ratio of 1:1.2:0.05:0.1, and stir evenly at room temperature to obtain a bio-based polyurethane adhesive for bamboo-wrapped composite pipes.
[0054] Example 3
[0055] Step 1: 18g of isophorone diisocyanate, 35g of vegetable oil-based polyol, 10g of dihydroxymethylbutyric acid, 100μL of stannous octoate and 30mL of acetone were added to a 250mL three-necked flask, nitrogen was introduced, and the mixture was heated to 85°C for 6h. The temperature was then lowered to 50°C, 7mL of triethylamine was added dropwise, and the reaction was continued for 1h. Finally, 180mL of deionized water was added and stirred for 1.5h, and the resulting emulsion was then rotary evaporated at 55°C to remove excess acetone to obtain a bio-based polyurethane emulsion with a solid content of approximately 25%;
[0056] Step 2: dissolving 30 g of soy protein in 85 mL of deionized water and stirring for 2 h to obtain a soy protein solution;
[0057] Step 3: Ultrasonic dispersion of the layered double hydroxide nanosheets in deionized water for 15 minutes to obtain a 10 mg / mL layered double hydroxide dispersion; then, polydopamine is dissolved in deionized water to obtain a 1 mg / mL polydopamine aqueous solution, and then the polydopamine aqueous solution is added dropwise to the layered double hydroxide dispersion, stirred at room temperature for 2 hours to obtain a layered double hydroxide @ polydopamine dispersion, and centrifuged and dried to obtain a layered double hydroxide @ polydopamine filler; the volume of the layered double hydroxide dispersion is 12 mL, and the volume of the tannic acid aqueous solution is 2 mL.
[0058] Step 4: blend the bio-based polyurethane emulsion, soy protein solution, layered double hydroxide@polydopamine filler, and diaminodiphenylmethane in a mass ratio of 1:1.5:0.1:0.15, and stir evenly at room temperature to obtain a bio-based polyurethane adhesive for bamboo-wrapped composite pipes.
[0059] The action mechanism of the green bio-based polyurethane adhesive for bamboo-wrapped pipes prepared by the present invention includes synergistic effects such as hydrogen bonding, physical adsorption and penetration, which enables it to form a strong bond with bamboo, provide excellent mechanical properties and durability, and at the same time improve the environmental friendliness of the adhesive.
Claims
1. A method for preparing a green bio-based polyurethane adhesive for bamboo winding pipes, characterized in that: The specific steps include: Step 1, adding aliphatic isocyanate, bio-based polyol, catalyst, chain extender and acetone into a reaction container in sequence, introducing nitrogen and heating and stirring to obtain a bio-based polyurethane prepolymer; Step 2, preparing a bio-based polyurethane emulsion according to the product obtained in step 1; Step 3, blending the bio-based polyurethane emulsion obtained in step 2 with the soybean protein solution, the curing agent, and the nanofiller modified with the polyphenol compound, and stirring evenly at room temperature to obtain the bio-based polyurethane adhesive for the bamboo-wrapped composite pipe.
2. The method for preparing the green bio-based polyurethane adhesive for bamboo winding pipe according to claim 1, characterized in that: In the step 1, the mass of the aliphatic isocyanate is 10-18 g, the mass of the bio-based polyol is 24-35 g, the mass of the catalyst is 50-100 μL, the mass of the chain extender is 3-10 g, and the volume of acetone is 30 mL.
3. The method for preparing the green bio-based polyurethane adhesive for bamboo winding pipe according to claim 2, characterized in that: In the step 1, the aliphatic isocyanate is one of hexamethylene diisocyanate, isophorone diisocyanate and trimethyl hexamethylene diisocyanate; The bio-based polyol is at least one of a plant oil-based polyol and a wood fiber-based polyol; The catalyst is at least one of dibutyltin dilaurate, stannous octoate, stannous oleate and lead isooctanoate; The chain extender is one of dimethylol propionic acid, dimethylol butyric acid, dihydroxy half ester, sodium ethylenediamine sulfonate and diethylenetriamine.
4. The method for preparing the green bio-based polyurethane adhesive for bamboo winding pipe according to claim 2, characterized in that: In the step 1, the heating temperature is 75-85° C. and the stirring time is 4-6 hours.
5. The method for preparing the green bio-based polyurethane adhesive for bamboo winding pipe according to claim 2, characterized in that: The specific process of step 2 is as follows: The temperature of the reaction container is reduced to 25-50° C., a salt-forming agent is added to the bio-based polyurethane prepolymer obtained in step 1 and stirred for 0.5-1 h to form salt, then 130-180 mL of deionized water is added and stirred for 0.5-1.5 h to emulsify, and finally rotary evaporation is performed at 55° C. to obtain a bio-based waterborne polyurethane emulsion.
6. The method for preparing the green bio-based polyurethane adhesive for bamboo winding pipe according to claim 5, characterized in that: In the step 2, the salt-forming agent is one of triethylamine, ammonia water and sodium hydroxide, and the amount of the salt-forming agent is 3-7 mL.
7. The method for preparing the green bio-based polyurethane adhesive for bamboo winding pipe according to claim 5, characterized in that: In step 3, the preparation method of the soy protein solution is: dissolving the soy protein in 70-85 mL of ionized water and stirring for 1-2 hours to obtain the soy protein solution, wherein the mass of the soy protein is 15-30 g.
8. The method for preparing the green bio-based polyurethane adhesive for bamboo-wound pipe according to claim 5, characterized in that: In step 3, the preparation process of the nanofiller modified with polyphenol compounds is as follows: The nanofiller is ultrasonically dispersed in deionized water for 15 minutes to obtain a 10 mg / mL nanofiller dispersion, and then the polyphenol compound is dissolved in deionized water to obtain a 1 mg / mL polyphenol compound aqueous solution, and then the polyphenol compound aqueous solution is added dropwise to the nanofiller dispersion, stirred at room temperature for 2 hours, and centrifuged to obtain a nanofiller powder modified with the polyphenol compound; the volume of the nanofiller dispersion is 8-12 mL, and the volume of the polyphenol compound aqueous solution is 0.5-2 mL.
9. The method for preparing a green bio-based polyurethane adhesive for bamboo-wrapped pipes according to claim 8, wherein in step 3, the mass ratio of the bio-based polyurethane emulsion: the soybean protein solution: the polyphenol-modified nanofiller: the curing agent is 1: 0.5-1.5: 0.01-0.1: 0.02-0.15; The curing agent is at least one of dicyandiamide, diaminodiphenylmethane and diaminodiphenyl sulfone; in, The polyphenol compound is one of tannic acid, gallic acid and polydopamine, and the nanofiller is one of lithium algae, zirconium hydrogen phosphate and layered double hydroxide; the polyphenol compound modified nanofiller is obtained.
10. Green bio-based polyurethane adhesive for bamboo winding pipe, characterized in that: The invention is prepared by adopting a preparation method of a green bio-based polyurethane adhesive for bamboo winding pipes.
Citation Information
Patent Citations
Aging-resistant polyurethane synthetic leather and production method thereof
CN104480738A
Preparation method of bio-based high-performance waterborne polyurethane resin and product thereof
CN112430308A
Preparation method of high-performance soybean protein adhesive
CN113061420A
Nano adhesive as well as preparation method and application thereof
CN113773796A
Hydrogen bond driven supramolecular assembled bio-based polyurethane flame-retardant coating and preparation method thereof