Forging method for uniformizing structure of large-specification 316H bar
Through the six-fire forging process, step by step cooling and water-cooling treatment, combined with low-temperature insulation forging, the problems of poor tissue uniformity and coarse grain size in 316H alloy forging were solved, and the grain size of the entire cross-section was significantly improved.
Patent Information
- Application Number
- CN202410963781.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing 316H alloy forging process has problems such as poor tissue uniformity and coarse grain size, which leads to inability to effectively improve performance.
Using the six-fire forging process, the heating temperature is reduced step by step, and water-cooled after the four-fire treatment, combined with the five-fire low-temperature and slow-frequency forging, to ensure the fine grain size and uniformity of the tissue, and at the same time, low-temperature insulation is carried out in the five-fire treatment. to restore the grain size at edge location.
Effectively refine the grain size of 316H alloy, improve the uniformity of the structure, and make the grain size of the full cross-section reach ≥3.0, with an extreme difference of ≤2.0, and solve the problem that the grain size in the existing process is generally between 0 and 1.5. the problem.
Smart Images

Figure CN118910377A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of forging, and in particular to a forging method for homogenizing the structure of a large-size 316H bar. Background Art
[0002] 316H alloy is a Cr-Ni-Mo iron-based alloy. It has good comprehensive properties such as high temperature strength, plasticity, toughness, corrosion resistance and weldability below 650℃. It has been widely used in various industries, especially in the field of nuclear power. Due to the composition of 316H alloy itself, there is no organizational transformation during the heat treatment process, and the grains cannot be uniformly refined. Therefore, the performance of 316H alloy mainly depends on the forging process.
[0003] At present, the conventional forging process for producing 316H alloy often adopts forging at 1180℃, and the finished product is obtained after three upsetting forgings. At this temperature, the grain size of the alloy core grows rapidly, generally at 0-1.5 levels, and the core grains are coarse. In addition, the forging process also has a series of problems such as poor uniformity of the obtained bar structure and elongated crystals on the surface, which in turn affects the performance of the product and makes it impossible to effectively improve the performance of the product. Therefore, it is necessary to develop a new production process for 316H alloy to improve its structural uniformity and refine the grains, thereby effectively improving the performance of 316H alloy. Summary of the invention
[0004] In view of the problems existing in the existing large-size 316H alloy forging process, such as poor organizational uniformity, coarse grain size, and inability to effectively improve performance, the present invention provides a forging method for homogenizing the organizational structure of large-size 316H bars.
[0005] To solve the above technical problems, the technical solution provided by the embodiment of the present invention is:
[0006] A forging method for homogenizing the structure of a large-size 316H bar comprises the following steps:
[0007] S1, heating the 316H electroslag ingot to a first fire treatment temperature, keeping the temperature and heating through, taking it out of the furnace, upsetting and drawing it to 880mm-900mm octagonal, and obtaining a first fire forging billet; wherein the first fire treatment temperature is 1170℃-1190℃;
[0008] S2, heating the first-fire forging billet to the second-fire treatment temperature, keeping the temperature to heat through, taking it out of the furnace for upsetting and stretching, and obtaining the second-fire forging billet; wherein the second-fire treatment temperature is 20°C to 30°C lower than the first-fire treatment temperature;
[0009] S3, heating the second-fire forging billet to the third-fire treatment temperature, keeping the temperature until it is heated through, taking it out of the furnace for upsetting and deformation, and obtaining the third-fire forging billet; wherein the third-fire treatment temperature is 50°C to 70°C lower than the second-fire treatment temperature;
[0010] S4, heating the three-fire forging billet to the four-fire treatment temperature, keeping the temperature to heat through, taking it out of the furnace for upsetting and drawing, and water cooling it to below 600° C. to obtain the four-fire forging billet; wherein the temperature of the four-fire treatment is the same as the temperature of the three-fire treatment;
[0011] S5, heating the four-fire forging billet at 980°C to 1000°C, then heating it to the five-fire treatment temperature, keeping it for 0.5h to 1h, and forging it to the finished product specifications at a frequency of 50% to 70%, to obtain the five-fire forging billet; wherein the five-fire treatment temperature is 30°C to 50°C lower than the four-fire treatment temperature;
[0012] S6, heating the five-fire forging billet to 1000° C.-1020° C., keeping the temperature for 40 min-60 min, taking it out of the furnace and air cooling it to obtain a 316H alloy rod.
[0013] Compared with the prior art, the forging method for homogenizing the microstructure of large-size 316H bars provided by the present invention adopts a method in which the heating temperature is gradually reduced along with the forging fires from the first fire to the third fire, and the temperature of the fourth fire is the same as the temperature of the third fire, and water cooling is performed after the fourth fire treatment, thereby effectively refining the grain size of the core of the 316H alloy; in addition, the fifth fire treatment adopts a low-temperature, slow-frequency forging method, which effectively reduces the temperature rise inside the bar, and is beneficial to further refine the grain size inside the 316H alloy and make the microstructure homogenized; finally, the fifth fire forging billet is kept at 1000°C to 1020°C for a specific time, thereby ensuring that the elongated crystals at the edge position are recovered and recrystallized, ensuring the uniformity of the grain size at the edge position, and completing a static recrystallization process for the grain size of the surface layer of the forging billet, thereby ensuring the grain uniformity of the entire cross section of 316H.
[0014] Specifically, the forging method for homogenizing the structure of large-size 316H bars provided by the present invention is suitable for preparing bars with a specification of Ф757mm to Ф760mm.
[0015] Furthermore, in S1, the 316H electroslag ingot is cylindrical with a diameter of 920 mm to 1020 mm.
[0016] It should be noted that the 316H electroslag ingot described in the present invention can be prepared by conventional methods in the art, such as electric furnace smelting, AOD refining, LF refining, VD vacuum refining, casting to obtain a Ф680mm electrode, and electroslag remelting to obtain a Ф920mm electroslag ingot.
[0017] Furthermore, in S1, the heat preservation and heating time is 6h to 8h.
[0018] Furthermore, in S1, the amount of deformation due to elongation is 35% to 45%.
[0019] Specifically, in S1, the steel bar is firstly roughened to a diameter of 1140 mm to 1160 mm and then stretched to an octagonal size of 880 mm to 900 mm.
[0020] Furthermore, in S2, the heat preservation and heating time is 2h to 3h.
[0021] Furthermore, in S2, the steel is firstly roughened to a diameter of 1140 mm to 1160 mm, and then stretched to an octagonal shape of 880 mm to 900 mm, and the amount of deformation during the stretching is 35% to 45%.
[0022] Furthermore, in S3, the deformation amount of the upset is 30% to 40%.
[0023] Specifically, in S3, the steel is roughened to a diameter of 1090 mm to 1110 mm.
[0024] Furthermore, in S3, the heat preservation and heating time is 4h to 6h.
[0025] Furthermore, in S4, the steel is firstly roughened to a diameter of 1210 mm to 1240 mm, and then stretched to a diameter of 1150 mm to 1180 mm, and the total deformation of the roughening and stretching is 20% to 40%.
[0026] Furthermore, in S4, the heat preservation and heating time is 2h to 3h.
[0027] Furthermore, in S5, the heat preservation and heating time is 4h to 5h.
[0028] Furthermore, in S5, the amount of deformation during forging is 45% to 60%.
[0029] The present invention adopts a forging method in which each deformation is greater than 25%, accompanied by a roughening process, which can ensure that the cast structure inside the forging billet is fully broken, and the core and radius have sufficient deformation, ensuring that the grains at the core and radius will not grow due to reheating in the next fire.
[0030] Specifically, the present invention can adopt a 6000-ton fast forging machine to produce a rod with uniform structure through the above 6-fire process. The grain size of the whole cross section of the 316H alloy rod forged by this process is ≥3.0 level, and the range is ≤2.0 level.
[0031] It should be noted that the above deformation amounts in the present invention all refer to the ratio of the cross-sectional areas before and after the plastic deformation.
[0032] The present invention also provides a large-size 316H bar, characterized in that it is prepared by the forging method for homogenizing the structure of the large-size 316H bar described in any one of the above items.
[0033] The forging method of large-size 316H bars provided by the present invention adopts a six-fire forging process, and the temperature is gradually reduced from the first fire to the third fire, the temperature of the fourth fire is the same as that of the third fire, and water cooling is performed after the fourth fire forging, and the fifth fire adopts a low-temperature and slow-frequency forging method, which effectively improves the organizational uniformity of the 316H bars, refines the grain size, and the grain size of the entire cross section is ≥3.0 levels, and the extreme difference is ≤2.0 levels, which effectively solves the problem that the grain size of the existing 316H alloy is generally 0-1.5 levels and the organizational homogenization is difficult, and the improved process is simple to operate and has high practical value. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the grain size sampling position in the embodiment;
[0035] Figure 2 The metallographic structure diagrams at the edge, 1 / 2 radius and center of the head and tail of the 316H rod prepared in Example 1; wherein A1 is the edge position of the head, A2 is the 1 / 2 radius position of the head, A3 is the center position of the head, B1 is the edge position of the tail, B2 is the 1 / 2 radius position of the tail, and B3 is the center position of the tail;
[0036] Figure 3 The metallographic structure diagrams at the edge, 1 / 2 radius and center of the head and tail of the 316H rod prepared in Comparative Example 1; wherein A1 is the edge position of the head, A2 is the 1 / 2 radius position of the head, A3 is the center position of the head, B1 is the edge position of the tail, B2 is the 1 / 2 radius position of the tail, and B3 is the center position of the tail. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] In order to better illustrate the present invention, further examples are given below.
[0039] Example 1
[0040] The embodiment of the present invention provides a forging method for homogenizing the structure of a large-size 316H bar, and the steps are as follows:
[0041] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1180℃, keep it warm for 7h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1150mm, then stretch it to 900mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0042] S2, heating the first-fire forging billet to 1150°C, keeping the temperature for 2 hours to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1150mm, and then drawing and forging it to 900mm octagonal, to obtain the second-fire forging billet;
[0043] S3, heating the second-fire forging billet to 1100°C, keeping the temperature for 5 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1100mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0044] S4, continue to heat the three-fire forging billet to 1100°C, keep it warm for 2 hours to make the steel ingot evenly heated, then take it out of the furnace, roughen it to a diameter of 1220mm, and then stretch it to a diameter of 1150mm. After forging, water cool it for 2 hours to make the billet temperature ≤600°C, and obtain the four-fire forging billet;
[0045] S5, reheating the four-fire forging billet to 1000°C and keeping it for 4 hours, then heating it to 1050°C and keeping it for 0.5 hours, taking it out of the furnace and subjecting it to drawing deformation at a forging frequency of 50% to obtain a round steel with a diameter of 757 mm;
[0046] S6, return the 757mm round steel to the furnace, heat it to 1010℃ and keep it at this temperature for 50 minutes, then take it out of the furnace and air cool it to obtain 316H bars.
[0047] Example 2
[0048] The embodiment of the present invention provides a forging method for homogenizing the structure of a large-size 316H bar, and the steps are as follows:
[0049] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1170℃, keep it warm for 8h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1140mm, then stretch it to 880mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0050] S2, heating the first-fire forging billet to 1140°C, keeping the temperature for 3 hours to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1140mm, and then drawing and forging it to 880mm octagonal, to obtain the second-fire forging billet;
[0051] S3, heating the second-fire forging billet to 1070°C, keeping the temperature for 6 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1090mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0052] S4, continue to heat the three-fire forging billet to 1070°C, keep it warm for 3 hours to make the steel ingot evenly heated, then take it out of the furnace, first roughen it to a diameter of 1210mm, then draw it to a diameter of 1160mm, and water cool it for 2 hours after forging to make the billet temperature ≤600°C, to obtain the four-fire forging billet;
[0053] S5, reheating the four-fire forging billet to 980°C and keeping it for 5 hours, then heating it to 1020°C and keeping it for 1 hour, taking it out of the furnace and subjecting it to drawing deformation at a forging frequency of 70% to obtain a 760mm round steel;
[0054] S6, return the 760mm round steel to the furnace, heat it to 1000℃ and keep it at this temperature for 60min, then take it out of the furnace and air cool it to obtain 316H bars.
[0055] Example 3
[0056] The embodiment of the present invention provides a forging method for homogenizing the structure of a large-size 316H bar, and the steps are as follows:
[0057] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1190℃, keep it warm for 6h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1160mm, then stretch it to 890mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0058] S2, heating the first-fire forging billet to 1170°C, keeping the temperature for 2 hours to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1160mm, and then drawing and forging it to 890mm octagonal, to obtain the second-fire forging billet;
[0059] S3, heating the second-fire forging billet to 1120°C, keeping the temperature for 4 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1110mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0060] S4, continue to heat the three-fire forging billet to 1120°C, keep it warm for 2 hours to make the steel ingot evenly heated, then take it out of the furnace, first roughen it to a diameter of 1240mm, then draw it to a diameter of 1180mm, and water cool it for 2 hours after forging to make the billet temperature ≤600°C, to obtain the four-fire forging billet;
[0061] S5, reheating the four-fire forging billet to 990°C for 4 hours, then heating it to 1090°C for 0.5 hours, taking it out of the furnace and subjecting it to drawing deformation at a forging frequency of 60% to obtain a 758mm round steel bar;
[0062] S6, return the 758mm round steel to the furnace, heat it to 1020℃ and keep it at this temperature for 40min, then take it out of the furnace and air cool it to obtain 316H bars.
[0063] Comparative Example 1
[0064] This comparative example provides a forging method for a large-size 316H bar. The only difference from Example 1 is that the temperature of the second fire is different from that of the fourth fire (that is, this comparative example adopts a method in which the first and second fires are isothermal, and the temperature of the third to fifth fires is gradually reduced), and no water cooling is performed after the fourth fire. The specific steps are as follows:
[0065] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1180℃, keep it warm for 7h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1150mm, then stretch it to 900mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0066] S2, heating the first-fire forging billet to 1180℃, keeping it warm for 2h to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1150mm, and then drawing and forging it to 900mm octagonal, to obtain the second-fire forging billet;
[0067] S3, heating the second-fire forging billet to 1100°C, keeping the temperature for 5 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1100mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0068] S4, continue to heat the three-fire forging billet to 1080℃, keep it warm for 2h to make the steel ingot evenly heated, then take it out of the furnace, first roughen it to a diameter of 1220mm, and then stretch it to a diameter of 1150mm, to obtain the four-fire forging billet;
[0069] S5, heating the four-fire forging billet to 1050°C, keeping the temperature for 3 hours, taking it out of the furnace and subjecting it to drawing deformation at a forging frequency of 50% to obtain a round steel with a diameter of 757 mm;
[0070] S6, return the 757mm round steel to the furnace, heat it to 1010℃ and keep it at this temperature for 50 minutes, then take it out of the furnace and air cool it to obtain 316H bars.
[0071] Comparative Example 2
[0072] This comparative example provides a forging method for a large-size 316H bar, which is different from Example 1 only in that no water cooling is performed after the fourth fire. The specific steps are as follows:
[0073] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1180℃, keep it warm for 7h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1150mm, then stretch it to 900mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0074] S2, heating the first-fire forging billet to 1150°C, keeping the temperature for 2 hours to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1150mm, and then drawing and forging it to 900mm octagonal, to obtain the second-fire forging billet;
[0075] S3, heating the second-fire forging billet to 1100°C, keeping the temperature for 5 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1100mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0076] S4, continue to heat the three-fire forging billet to 1100°C, keep it warm for 2 hours to make the steel ingot evenly heated, then take it out of the furnace, first roughen it to a diameter of 1220mm, and then stretch it to a diameter of 1150mm, to obtain the four-fire forging billet;
[0077] S5, reheating the four-fire forging billet to 1000°C and keeping it for 4 hours, then heating it to 1050°C and keeping it for 0.5 hours, taking it out of the furnace and subjecting it to drawing deformation at a forging frequency of 50% to obtain a round steel with a diameter of 757 mm;
[0078] S6, return the 757mm round steel to the furnace, heat it to 1010℃ and keep it at this temperature for 50 minutes, then take it out of the furnace and air cool it to obtain 316H bars.
[0079] Comparative Example 3
[0080] This comparative example provides a forging method for a large-size 316H bar. The only difference from Example 1 is that an air cooling step is added after the second and fourth fires. The specific steps are as follows:
[0081] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1180℃, keep it warm for 7h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1150mm, then stretch it to 900mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0082] S2, heating the first-fire forging billet to 1150°C, keeping it warm for 2 hours to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1150mm, then drawing and forging it to 900mm octagonal, and then air cooling it until the surface temperature of the forging billet reaches 600-700°C, so as to obtain the second-fire forging billet;
[0083] S3, heating the second-fire forging billet to 1100°C, keeping the temperature for 5 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1100mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0084] S4, continue to heat the three-fire forging billet to 1100℃, keep it warm for 2h to make the steel ingot evenly heated, then take it out of the furnace, roughen it to a diameter of 1220mm, then draw it to a diameter of 1150mm, and then air cool it until the surface temperature of the forging billet reaches 600-700℃, so as to obtain the four-fire forging billet;
[0085] S5, reheating the four-fire forging billet to 1000°C and keeping it for 4 hours, then heating it to 1050°C and keeping it for 0.5 hours, taking it out of the furnace and subjecting it to drawing deformation at a forging frequency of 50% to obtain a round steel with a diameter of 757 mm;
[0086] S6, return the 757mm round steel to the furnace, heat it to 1010℃ and keep it at this temperature for 50 minutes, then take it out of the furnace and air cool it to obtain 316H bars.
[0087] Comparative Example 4
[0088] This comparative example provides a forging method for a large-size 316H bar. The difference from Example 1 is that the first, second and third fires are performed in an isothermal manner, and an air cooling step is added after the second fire. The specific steps are as follows:
[0089] S1, heat a 316H electroslag ingot with a diameter of 920mm to 1180℃, keep it warm for 7h to make the ingot evenly heated, then take it out of the furnace, first upset it to a diameter of 1150mm, then stretch it to 900mm octagonal, and make a fire forging billet; in the upset process, first upset it 300mm, then stay for 20s and then continue upset;
[0090] S2, heating the first-fire forging billet to 1180℃, keeping it warm for 2h to make the steel ingot evenly heated, and then taking it out of the furnace, roughening it to a diameter of 1150mm, then drawing and forging it to 900mm octagonal, and then air cooling it until the surface temperature of the forging billet reaches 600-700℃, so as to obtain the second-fire forging billet;
[0091] S3, heating the second-fire forging billet to 1180°C, keeping the temperature for 2 hours to make the steel ingot evenly heated through, and then roughening it to a diameter of 1100mm after it is taken out of the furnace to obtain the third-fire forging billet;
[0092] S4, continue to heat the three-fire forging billet to 1050°C, keep the temperature for 3 hours, take it out of the furnace and make a round steel with a diameter of 760 mm by stretching and deformation at a forging frequency of 50%;
[0093] S6, return the 760mm round steel to the furnace, heat it to 1010℃ and keep it at this temperature for 50min, then take it out of the furnace and air cool it to obtain 316H bars.
[0094] Grain size test
[0095] The 316H bars with a diameter of 757 mm to 760 mm prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to multi-point inspection of grain size. In order to ensure that the test results are accurate and reliable, Figure 1 The sampling is carried out by the method shown, that is, multi-point sector sampling is adopted along the radius of the bar, and the test results are shown in Table 1.
[0096] Table 1 Grain size test results
[0097]
[0098]
[0099]
[0100] Note: The grain size expressions X(Y) and XY in the table are explained as follows: ①X(Y), representing that more than 90% of the grain size is X grade, and less than 10% is Y grade; ②X-Y, representing that there are mixed crystals in the structure, the matrix is X grade, accounting for >50%, and the rest is Y grade grain size.
[0101] It can be seen from the above table that although the grain size of the core is improved in Comparative Examples 1 to 3, the finished products all have large grains in the core. The embodiment of the present invention adopts a unique six-fire forging process, which can ensure that the internal structure of large-size 316H alloy bars is uniform, the grain size reaches above level 3.0, and the extreme difference is ≤ level 2.0 by controlling the temperature of each fire treatment, adding water cooling after four fires, and five-fire low-temperature, slow-frequency forging, and six-fire low-temperature insulation.
[0102] Figure 2 The metallographic structure diagrams at the edge, 1 / 2 radius and center of the head and tail of the 316H rod prepared in Example 1 are as follows: Figure 3 The metallographic structures at the edge, 1 / 2 radius and center of the head and tail of the 316H rod prepared in Comparative Example 1 are shown.
[0103] As can be seen from the figure, there are elongated crystals at the edge of the head and tail of Comparative Example 1, the level is greater than level 0, the fine crystals can reach level 7.0, and the grain size at the 1 / 2 radius can mostly meet the requirements of ≥ level 3.0, but there are individual large grains, and the grain size at the center is between 0 and 1.5. The grain sizes at the edges of the head and tail, the 1 / 2 radius and the center of the 316H rod prepared in Example 1 are all between 3.0 and 4.0, and are evenly distributed, meeting the requirements.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A forging method for homogenizing the structure of large-size 316H bars, characterized in that: The steps include: S1, heating the 316H electroslag ingot to a first fire treatment temperature, keeping the temperature and heating through, taking it out of the furnace, upsetting and drawing it to 880mm-900mm octagonal, and obtaining a first fire forging billet; wherein the first fire treatment temperature is 1170℃-1190℃; S2, heating the first-fire forging billet to the second-fire treatment temperature, keeping the temperature to heat through, taking it out of the furnace for upsetting and stretching, and obtaining the second-fire forging billet; wherein the second-fire treatment temperature is 20°C to 30°C lower than the first-fire treatment temperature; S3, heating the second-fire forging billet to the third-fire treatment temperature, keeping the temperature until it is heated through, taking it out of the furnace for upsetting and deformation, and obtaining the third-fire forging billet; wherein the third-fire treatment temperature is 50°C to 70°C lower than the second-fire treatment temperature; S4, heating the three-fire forging billet to the four-fire treatment temperature, keeping the temperature to heat through, taking it out of the furnace for upsetting and drawing, and water cooling it to below 600° C. to obtain the four-fire forging billet; wherein the temperature of the four-fire treatment is the same as the temperature of the three-fire treatment; S5, heating the four-fire forging billet at 980°C to 1000°C, then heating it to the five-fire treatment temperature, keeping it for 0.5h to 1h, and forging it to the finished product specifications at a frequency of 50% to 70%, to obtain the five-fire forging billet; wherein the five-fire treatment temperature is 30°C to 50°C lower than the four-fire treatment temperature; S6, heating the five-fire forging billet to 1000° C.-1020° C., keeping the temperature for 40 min-60 min, taking it out of the furnace and air cooling it to obtain a 316H alloy rod.
2. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S1, the 316H electroslag ingot is cylindrical with a diameter of 920 mm to 1020 mm; and / or In S1, the heat preservation and heating time is 6h to 8h; and / or In S1, the amount of deformation by drawing is 35% to 45%.
3. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S2, the heat preservation and heating time is 2h to 3h; and / or In S2, the steel is firstly roughened to a diameter of 1140 mm to 1160 mm, and then stretched to an octagonal shape of 880 mm to 900 mm, with a deformation amount of 35% to 45%.
4. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S3, the deformation of the upsetting is 30% to 40%; and / or In S3, the heat preservation and heating time is 4h to 6h.
5. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S4, the steel is firstly roughened to a diameter of 1210 mm to 1240 mm, and then stretched to a diameter of 1150 mm to 1180 mm. The total deformation of roughening and stretching is 20% to 40%.
6. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S4, the heat preservation and heating time is 2h to 3h.
7. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S5, the heat preservation and heating time is 4h to 5h.
8. The forging method for homogenizing the structure of large-size 316H bars according to claim 1, characterized in that: In S5, the diameter of the finished product is 757 mm to 760 mm.
9. The forging method for homogenizing the structure of a large-size 316H bar as claimed in claim 8, characterized in that: In S5, the amount of deformation during forging is 45% to 60%.
10. A large-size 316H bar, characterized in that: The large-size 316H bar is prepared by the forging method for homogenizing the structure of the large-size 316H bar as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Forging control method for uniformly refining grain sizes of forgings
CN110684885A
GH738 high-temperature alloy grain homogenization forging technology
CN112828219A
GH4169 alloy wide and flat billet structure homogenization forging process
CN114309409A
Method for controlling rolling grain size of 316H austenitic stainless steel medium plate for nuclear power
CN114891994A
Preparation method of high-temperature alloy bar billet for thermal power generating unit valve
CN117051217A
Cited By
Forging method of large-size high-temperature alloy bar
CN121945667A