Method for controlling heat treatment buckling deformation of large forge piece shaped like Chinese character'ri '

By setting up support structures and pads in the material preparation, heating and air-cooling links of forgings, the deformation of forgings is controlled, and the problem of warping and bending deformation during the heat treatment of forgings is solved, which improves the quality of forgings and reduces manufacturing costs.

CN118910385APending Publication Date: 2024-11-08CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411333239.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the heat treatment of forgings, due to factors such as heating temperature and gravity, large shaped forgings are warped, bending and deformed, affecting their quality and increasing manufacturing costs.

Method used

By setting up a support structure in the material preparation link to control the horizontal support of the forging, avoid deformation caused by direct lifting, and use hanging points and pads for suspended support in the heating and air-cooling links, setting deformation and giving way gaps to compensate for deformation, ensuring that the forging is in The deformation during heat treatment is within a reasonable range.

Benefits of technology

It effectively avoids the middle upper deformation of the forging during the heat treatment process, reduces the upper deformation of the later stage of cooling, improves the quality of the forging and reduces the manufacturing cost, and avoids subsequent calibration needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910385A_ABST
    Figure CN118910385A_ABST
Patent Text Reader

Abstract

The invention provides a method for controlling the heat treatment buckling deformation of a large-sized Chinese character ri-shaped forge piece, which is used for conveniently controlling the buckling deformation of the large-sized Chinese character ri-shaped forge piece in the heat treatment process to be within a required reasonable range so as to improve the quality of the forge piece and reduce the manufacturing cost of the forge piece, and relates to the technical field of heat treatment deformation treatment of the forge piece. According to the method for controlling heat treatment buckling deformation of the large forge piece shaped like the Chinese character'ri ', material preparation link control comprises the steps that in the material preparation process, the first support, the second support and the third support serve as main force bearing supports, and the forge piece is horizontally supported on a material disc; the air cooling link control comprises the steps that when a forge piece is placed on the cooling material frame, the forge piece is suspended and horizontally supported on the cooling material frame in the mode that a left frame and a right frame are supported; and a deformation receding gap A capable of enabling the middle of the forge piece to deform downwards in the early cooling stage so as to compensate upward arching deformation in the later cooling stage is reserved between the forge piece and the cooling material frame.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of forging heat treatment deformation treatment, and specifically to a method for controlling the warping deformation of large-sized H-shaped forgings during heat treatment. Background Art

[0002] During the heat treatment of forgings, it includes three links: stock preparation, heat treatment, and air cooling. During the heat treatment of forgings, the heating temperature is high. Under the influence of various complex factors such as temperature stress and the self-gravity of the forgings, the forgings will undergo self-warping and bending deformation, seriously affecting the quality of the forgings.

[0003] As Figure 1 shown, the H-shaped forging 1 includes a left frame 11, a front frame 12, a right frame 13, and a rear frame 14 that are sequentially connected end to end to enclose a square frame, and further includes a cross bar 15 disposed within the square frame and connected at one end to the middle of the front frame 12 and at the other end to the middle of the right frame 13 to divide the square frame into an H-shaped structure. As Figure 1 shown, for large-sized H-shaped forgings with a length greater than 3 meters, in order to ensure the balance of the forgings during the heat treatment hoisting and transportation process, the existing method is to respectively set two lifting points 16 close to the cross bar on both sides of the cross bar 15. The two lifting points on one side are symmetrically arranged with respect to the cross bar 15 with the two lifting points on the other side. For the two lifting points on the same side, one is located on the front frame 12 and the other is located on the rear frame 14, and then the forging is hoisted and transported through the four above-mentioned lifting points. The lifting points 16 are close to the cross bar, that is, the distance from the left lifting point to the cross bar is less than the distance from this lifting point to the left frame 11, and the distance from the right lifting point to the cross bar is less than the distance from this lifting point to the right frame 13. During the heat treatment hoisting and transportation process of the forging, affected by the gravity at both ends, the forging will generate a deformation of upward arching in the middle, resulting in difficulties in subsequent correction of the forging, not only affecting the quality of the forging, but also increasing the manufacturing cost of the forging. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a method for controlling the warping deformation of large-sized H-shaped forgings during heat treatment, so as to facilitate the control of the warping deformation during the heat treatment of large-sized H-shaped forgings, make it within the required reasonable range, thereby improving the quality of the forgings and reducing the manufacturing cost thereof.

[0005] The technical solution adopted by the present invention to solve its technical problems is: a method for controlling the warping deformation of large-sized H-shaped forgings during heat treatment, the forging includes a left frame, a front frame, a right frame, and a rear frame that are sequentially connected end to end to enclose a square frame, and further includes a cross bar disposed within the square frame and connected at one end to the middle of the front frame and at the other end to the middle of the right frame to divide the square frame into an H-shaped structure, the method includes control of the stock preparation link, control of the heat treatment link, and control of the air cooling link;

[0006] The material preparation link control includes: in the material preparation process, support one is set at the connecting corner of the left frame and the front frame, support two is set at the connecting corner of the front frame and the right frame, support three is set at one end of the rear frame and at a distance c from the cross bar, c is greater than or equal to one quarter of the length of the rear frame and less than one half of the length of the rear frame, and the forging is horizontally supported on the material tray with the support one, support two and support three as the main load-bearing supports; an auxiliary support is respectively set at one quarter of the length of the front frame, one half of the length of the front frame, three quarters of the length of the front frame, the midpoint of the left frame, the midpoint of the right frame, the other end of the rear frame and at a distance of one quarter of the length of the rear frame from the cross bar, the connecting corner of the rear frame and the right frame, and the connecting corner of the rear frame and the left frame, and a gap is set between the auxiliary support and the forging, and the gap is less than 1mm;

[0007] The control of the heating treatment process includes: during the heating treatment process, the forging is sent into and out of the heating furnace by hoisting the material tray with a hoisting device to perform the heating treatment, thereby avoiding deformation of the forging due to direct hoisting of the forging during the heating treatment process;

[0008] The air cooling link control includes: hoisting and transferring the forging to the cooling rack for air cooling through four hoisting points symmetrically arranged on both sides of the cross bar and arranged close to the cross bar, wherein, when the forging is placed on the cooling rack, the forging is suspended and horizontally supported on the cooling rack by supporting the left frame and the right frame with a pad 1 arranged under the left frame and a pad 2 arranged under the right frame, so that a deformation clearance gap A is left between the forging and the cooling rack to allow the middle part of the forging to deform downward in the early stage of cooling to compensate for the upward arch deformation in the later stage of cooling.

[0009] Furthermore, the deformation clearance gap A=B-4, wherein B is the theoretical arch deformation amount of the forging.

[0010] Furthermore, the pad block 1 consists of three pieces, one of which is set at half the length of the left frame, one of which is set at the connection between the left frame and the front frame, and one of which is set at the connection between the left frame and the rear frame; the pad block 2 also consists of three pieces, one of which is set at half the length of the right frame, one of which is set at the connection between the right frame and the front frame, and one of which is set at the connection between the right frame and the rear frame.

[0011] Furthermore, the cooling rack is a Japanese-shaped bracket designed according to the shape of the forging.

[0012] Further, c is equal to one quarter of the length of the rear border.

[0013] The beneficial effects of the present invention are as follows: A method for controlling the heat treatment warping deformation of a large-sized rectangular forging of the present invention includes control of the stock preparation link, control of the heat treatment link, and control of the air cooling link. In the control of the stock preparation link, the middle position of the forging has a tendency to bend downward under the action of gravity, so that the forging can produce a certain downward deformation or deformation tendency as the temperature rises during the heat treatment link, thereby avoiding the upward deformation in the middle of the forging and also being beneficial to reducing the upward deformation during the cooling, hoisting, and transportation of the forging. In the control of the air cooling link, the forging is suspended and supported on the material rack through the cushion blocks 31 at both ends and the cushion blocks 32. There is a deformation allowance gap A for deformation compensation between the forging and the material rack. Through the gap A between the forging and the cooling material rack, the middle part of the forging can deform downward when the forging material is relatively soft in the early stage of cooling, so as to supplement the upward deformation amount of the forging in the later stage of cooling through this deformation, so that the forging finally does not deform or deforms within the required range, thereby making the forging not require correction in the later stage, improving the quality of the forging, and reducing its manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is a schematic structural diagram of the forging of the present invention;

[0015] Figure 2 is a schematic diagram of the support setting during forging stock preparation;

[0016] Figure 3 is a schematic diagram of the support setting during forging cooling;

[0017] Figure 4 is a schematic structural diagram of the material rack;

[0018] As shown in the figure: forging 1, material tray 2, cooling material rack 3, left frame 11, front frame 12, right frame 13, rear frame 14, cross bar 15, lifting point 16, support 17, support 18, support 19, auxiliary support 20, cushion block 31, cushion block 32. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0019] The present invention will be further described below in conjunction with the drawings and embodiments.

[0020] As Figures 1 to 4 shown, a method for controlling the heat treatment warping deformation of a large-sized rectangular forging of the present invention, the forging 1 includes a left frame 11, a front frame 12, a right frame 13, and a rear frame 14 that are sequentially connected end to end and enclose a square frame, and further includes a cross bar 15 disposed within the square frame and connected to the middle of the front frame 12 at one end and the middle of the right frame 13 at the other end to divide the square frame into a rectangular structure. The method includes control of the stock preparation link, control of the heat treatment link, and control of the air cooling link.

[0021] The material preparation link control includes: in the material preparation process, support one 17 is set at the connection corner of the left frame 11 and the front frame 12, support two 18 is set at the connection corner of the front frame 12 and the right frame 13, and support three 19 is set at one end of the rear frame 14 and at a distance c from the cross bar 15, where c is greater than or equal to one quarter of the length of the rear frame 14 and less than one half of the length of the rear frame 14, and the forging 1 is horizontally supported on the material tray 2 with the support one 17, the support two 18 and the support three 19 as the main load-bearing supports; on the front frame 1 2, one-half the length of the front frame 12, three-quarters the length of the front frame 12, the midpoint of the left frame 11, the midpoint of the right frame 13, the other end of the rear frame 14 and the distance from the cross bar 15 is one-quarter the length of the rear frame 14, the connecting corner of the rear frame 14 and the right frame 13, and the connecting corner of the rear frame 14 and the left frame 11, respectively, an auxiliary support 20 is set, and a gap is set between the auxiliary support 20 and the forging 1, and the gap is less than 1mm.

[0022] The control of the heating treatment process includes: during the heating treatment process, the forging 1 is sent into and out of the heating furnace for heating treatment by hoisting the material tray 2 with a hoisting device, thereby avoiding deformation of the forging due to direct hoisting of the forging during the heating treatment process.

[0023] The air cooling link control includes: hoisting and transferring the forging to the cooling rack 3 for air cooling through four hanging points 16 symmetrically arranged on both sides of the cross bar 15 and arranged close to the cross bar. The setting position of the hanging points 16 is the same as the existing method. In order to control the subsequent deformation of the forging, when the forging is placed on the cooling rack 3, the pad 1 31 arranged under the left frame 11 and the pad 2 32 arranged under the right frame 13 are used to support the left frame 11 and the right frame 13 to support the forging 1 horizontally on the cooling rack 3 in the air, so that a deformation clearance gap A is left between the forging 1 and the cooling rack 3, which allows the middle part of the forging 1 to deform downward in the early cooling stage to compensate for the upward arch deformation in the late cooling stage.

[0024] In the embodiment of the present invention, a is equal to one quarter of the length of the rear frame 14 , that is, the support three 19 is arranged at one end of the rear frame 14 and the distance from the cross bar 15 is equal to one quarter of the length of the rear frame 14 .

[0025] The auxiliary support 20 is generally provided in the following manner:

[0026] Step 1: Set support 1 17, support 2 18 and support 3 19 on the material tray;

[0027] Step 2: Place the forging on support 1 17, support 2 18 and support 3 19, so that the forging is horizontally supported on the tray by support 1 17, support 2 18 and support 3 19;

[0028] Step 3: Arrange an auxiliary support column at a corresponding position on the material tray, with a gap between the upper end of the auxiliary support column and the forging;

[0029] Step 4: Insert gaskets between the auxiliary support column and the forging respectively until the gap between the auxiliary support 20 and the forging 1 is less than 1 mm.

[0030] The method for controlling the warping deformation of large-scale Chinese-Japanese-shaped forgings during heat treatment of the present invention is as follows: in the material preparation stage, support 1 17 is provided at the connecting corner between the left frame 11 and the front frame 12, support 2 18 is provided at the connecting corner between the front frame 12 and the right frame 13, and support 3 19 is provided at one end of the rear frame 14 and at a distance c from the crossbar 15, where c is greater than or equal to one-fourth of the length of the rear frame 14 and less than one-half of the length of the rear frame 14. With support 1 17, support 2 18 and support 3 19 as the main load-bearing supports, the forging 1 is horizontally supported on the material tray 2, which not only ensures the support stability of the forging, but also makes the middle position of the forging have a tendency to bend and deform downward under the action of gravity, so that the forging can produce a certain downward deformation or deformation tendency as the temperature rises during the heating treatment stage, thereby avoiding the upward deformation in the middle of the forging, and also helps to reduce the upward deformation of the forging during cooling, hoisting and transportation. The auxiliary support 20 can control the downward deformation of the forging, especially the middle part of the forging. During cooling, the forging 1 is suspended horizontally on the cooling rack 3 by means of the pad 1 31 arranged under the left frame 11 and the pad 2 32 arranged under the right frame 13, so that a deformation clearance gap A is left between the forging 1 and the cooling rack 3, which allows the middle part of the forging 1 to deform downward in the early cooling stage to compensate for the upward deformation in the late cooling stage. Through the gap A, the middle part of the forging can be deformed downward when the forging material is relatively soft in the early cooling stage, so as to supplement the upward deformation of the forging in the late cooling stage through the deformation, so that the forging is not deformed or deformed within the required range in the end. The various control links of the method of the present invention cooperate with each other, and the forging obtained does not need to be corrected in the later stage, which improves the quality of the forging and reduces the manufacturing cost.

[0031] Through experiments, it is found that optimally, the deformation clearance gap A=B-4, wherein B is the theoretical arch deformation amount of the forging 1.

[0032] The number and position of the pad 1 31 and the pad 2 32 can be freely set. In the present invention, in order to stably support the forging and facilitate its cooling, the pad 1 31 is preferably three blocks, one of which is set at half the length of the left frame 11, one of which is set at the connection between the left frame 11 and the front frame 12, and one of which is set at the connection between the left frame 11 and the rear frame 14; the pad 2 32 is also three blocks, one of which is set at half the length of the right frame 13, one of which is set at the connection between the right frame 13 and the front frame 12, and one of which is set at the connection between the right frame 13 and the rear frame 14.

[0033] In order to facilitate accurate placement of the forgings on the cooling rack according to the position of the pad support, a positioning structure that cooperates with the forgings can be provided on the cooling rack as needed.

[0034] The cooling rack 3 can adopt various existing structural racks. In order to utilize the cooling of the forging and control the deformation of the forging, in the present invention, the cooling rack 3 is preferably a Japanese-shaped bracket designed according to the shape of the forging 1. Of course, in order to increase the strength of the Japanese-shaped bracket, it can also be changed into a field-shaped structure.

Claims

1. A method for controlling the heat treatment warping deformation of a large-sized rectangular forging. The forging includes a left frame (11), a front frame (12), a right frame (13), and a rear frame (14) that are sequentially connected end to end to form a square frame, and further includes a cross bar (15) disposed within the square frame and connected at one end to the middle of the front frame (12) and at the other end to the middle of the right frame (13) to divide the square frame into a rectangular structure. The method is characterized in that, The method includes material preparation link control, heating treatment link control and air cooling link control; The material preparation link control comprises: in the material preparation process, a support 1 (17) is arranged at the connection corner between the left frame (11) and the front frame (12), a support 2 (18) is arranged at the connection corner between the front frame (12) and the right frame (13), and a support 3 (19) is arranged at one end of the rear frame (14) and at a distance c from the cross bar (15), where c is greater than or equal to one quarter of the length of the rear frame (14) and less than one half of the length of the rear frame (14), and the support 1 (17), the support 2 (18) and the support 3 (19) are used as the main load-bearing supports to horizontally support the forging on the material tray (2); at the front frame ( An auxiliary support (20) is respectively provided at a quarter of the length of the front frame (12), at a half of the length of the front frame (12), at three quarters of the length of the front frame (12), at the midpoint of the left frame (11), at the midpoint of the right frame (13), at the other end of the rear frame (14) and at a distance from the cross bar (15) of a quarter of the length of the rear frame (14), at a connecting corner between the rear frame (14) and the right frame (13), and at a connecting corner between the rear frame (14) and the left frame (11), and a gap is provided between the auxiliary support (20) and the forging, and the gap is less than 1 mm; The control of the heating treatment process comprises: during the heating treatment process, using a lifting device to lift the material tray (2) to send the forging into and out of the heating furnace for heating treatment, thereby avoiding deformation of the forging due to direct lifting of the forging during the heating treatment process; The air cooling control comprises: hoisting and transferring the forging to a cooling rack (3) for air cooling through four hoisting points (16) symmetrically arranged on both sides of a cross bar (15) and arranged close to the cross bar, wherein when the forging is placed on the cooling rack (3), a pad 1 (31) arranged under the left frame (11) and a pad 2 (32) arranged under the right frame (13) are used to suspend the forging and horizontally support it on the cooling rack (3) by supporting the left frame (11) and the right frame (13), so that a deformation clearance gap A is left between the forging and the cooling rack (3) so that the middle part of the forging can deform downward in the early cooling stage to compensate for the upward deformation in the late cooling stage.

2. The method for controlling the heat treatment warping deformation of a large-sized rectangular forging according to claim 1, characterized in that, The deformation clearance gap A=B-4, wherein B is the theoretical arch deformation amount of the forging.

3. The method for controlling the heat treatment warping deformation of a large-sized rectangular forging according to claim 1, characterized in that, The cushion block 1 (31) consists of three pieces, one of which is arranged at half the length of the left frame (11), one of which is arranged at the connection between the left frame (11) and the front frame (12), and one of which is arranged at the connection between the left frame (11) and the rear frame (14); the cushion block 2 (32) also consists of three pieces, one of which is arranged at half the length of the right frame (13), one of which is arranged at the connection between the right frame (13) and the front frame (12), and one of which is arranged at the connection between the right frame (13) and the rear frame (14).

4. The method for controlling the heat treatment warping deformation of a large-sized rectangular forging according to claim 1, characterized in that, The cooling rack (3) is a Japanese-shaped rack designed according to the shape of the forging.

5. The method for controlling the heat treatment warping deformation of a large-sized rectangular forging according to claim 1, characterized in that, c is equal to one quarter of the length of the rear frame (14).