Utilization method of iron ore through pneumatic classification, strong magnetic tailing discarding and suspension roasting in advance
Through pre-pneumatic grading and strong magnetic tailing throwing process of iron ore, combined with suspended roasting and hydrogen-based reduction, the problems of long and high heat consumption of iron ore treatment processes in the existing technology are solved, efficient iron concentrate production is achieved, and iron is improved total recovery rate and stability of product indicators.
Patent Information
- Application Number
- CN202410980215.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing iron ore treatment technology has problems such as long process, high grinding unit consumption, high selection cost and poor product indicators. In particular, the efficient use of low-grade weak magnetic ore is greatly affected by heat consumption.
Pre-pneumatic grading-strong magnetic tail-throwing-suspended roasting method is adopted to obtain fine and coarse-grained products through pneumatic grading, magnetic separation and roasting are performed respectively, and high-temperature roasting and suspended hydrogen-based reduction are performed after the merger, and further grinding is carried out. -Magnetic separation, obtain iron concentrate products with iron grade greater than 65%.
It has achieved efficient comprehensive utilization of iron ore, reduced heat consumption, improved the total recovery rate of iron, stable product indicators, good economy, and achieved the goal of "reducing costs and increasing efficiency".
Smart Images

Figure CN118910399A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting. Background Art
[0002] my country has abundant iron ore resources, but the reserves of high-quality iron ore are small, and the reserves of easily selected magnetite are low. Most of them are weakly magnetic ores such as low-grade hematite, limonite, siderite, and specularite. The domestic beneficiation methods for processing low-grade weakly magnetic ores are mainly grinding, magnetic separation, gravity separation, and flotation, which have problems such as long process, high grinding unit consumption, high separation cost, and poor product indicators.
[0003] As an emerging technology, suspended magnetization roasting technology can transform weakly magnetic iron minerals into strong magnetic iron minerals under certain temperature and atmosphere conditions, so that iron ore can be efficiently recovered using weak magnetism. Since this technology consumes heat energy, there is a large amount of heat consumption, which has a certain impact on the efficient utilization of iron ore. Summary of the invention
[0004] In view of the problems existing in the efficient utilization of existing iron ore, the present invention provides a new method for producing iron concentrate by pre-pneumatic classification of iron ore-strong magnetic tailings discarding-suspended roasting. The purpose is to pre-classify the iron ore, carry out strong magnetic tailings discarding of coarse-grained products, combine the obtained mixed concentrate with the fine-grained products, and then carry out high-temperature roasting and suspended hydrogen-based reduction, and then carry out grinding-magnetic separation to obtain an iron concentrate product with an iron grade greater than 65%.
[0005] A method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting is carried out according to the following steps:
[0006] (1) crushing the iron ore to a particle size of ≤30 mm and then performing pneumatic classification to obtain a fine-grained product and a coarse-grained product; the particle size of the fine-grained product is ≤3 mm, and the coarse-grained product is crushed-grinded to a particle size of ≤3 mm to obtain a crushed product; the crushed product is subjected to magnetic separation, firstly weak magnetic separation is performed to obtain a weak magnetic separation concentrate and a weak magnetic separation tailing, and then the weak magnetic separation tailing is subjected to strong magnetic separation to obtain a strong magnetic separation concentrate and a strong magnetic separation tailing, and the weak magnetic separation concentrate and the strong magnetic separation concentrate are combined as a coarse concentrate product, and the strong magnetic tailing is a qualified tailing;
[0007] (2) feeding the mixed ore obtained by mixing the fine-grained product with the coarse concentrate product into a suspension roasting furnace, gradually heating it for high-temperature roasting to remove impurities such as crystal water in the mixed ore, then placing it in a suspended state under a hydrogen-based reducing atmosphere for heat preservation, and then cooling it to 200-300° C. under a nitrogen atmosphere in the absence of oxygen, and then cooling it to 50-100° C. by introducing air to obtain a roasted ore;
[0008] (3) The roasted ore is passed into water to form a slurry and then subjected to magnetic separation to obtain a weak magnetic separation concentrate and a segment weak magnetic separation tailings, wherein the magnetic separation concentrate is used as an iron ore concentrate product and the weak magnetic separation tailings are used as qualified tailings.
[0009] Furthermore, the iron grade of the iron ore is 20% to 35%, and the particle size is greater than 10 mm.
[0010] Furthermore, in the magnetic separation method described in step (1), the magnetic force range of weak magnetic separation is 0.1-0.3T, and the magnetic force range of strong magnetic separation is 0.4-0.6T.
[0011] Furthermore, the high temperature roasting temperature in step (2) is 550-650° C., and the time is 2-10 seconds; the temperature of the suspension insulation is 500-540° C., and the insulation time is 10-30 minutes.
[0012] Furthermore, the reducing atmosphere in step (2) is a carbon monoxide atmosphere, a hydrogen atmosphere, or a coal gas atmosphere.
[0013] Furthermore, the iron grade of the coarse-grained product strong magnetic separation tailings in step (1) is 3% to 7%.
[0014] Furthermore, the iron grade of the mixed ore in step (2) is 30% to 45%, and the iron grade of the roasted ore is 32% to 47%.
[0015] Furthermore, the weight concentration of the slurry in step (3) is 40% to 70%.
[0016] Furthermore, the magnetic force range of the magnetic separation in step (3) is 0.1 to 0.4T.
[0017] Furthermore, the iron ore concentrate product in step (3) has an iron grade of more than 65%, and a total iron recovery rate of more than 90%; and the iron grade of the weak magnetic separation tailings is 3% to 8%.
[0018] The main physical and chemical reactions of the above invention are:
[0019] Fe2O3·nH2O→Fe2O3+H2O (1)
[0020] Fe2O3+H2→Fe3O4+H2O, Fe2O3+CO→Fe3O4+CO2 (2)
[0021] Fe3O4+O2→γ-Fe2O3 (3).
[0022] Compared with the prior art, the characteristics and beneficial effects of the present invention are:
[0023] The method of the present invention is to remove a part of the tailings products through the pre-classification-strong magnetic tailings discarding process, and the other products are mixed and then subjected to high-temperature roasting and suspended state reduction, wherein the purpose of pre-classification is:
[0024] (1) Using gas at a certain flow rate to classify the ore according to the iron content and material particle size, different process treatments are carried out for different classified materials, the coarse-grained products are subjected to strong magnetic separation, a part of the tailings are discarded, and the fine-grained products are directly subjected to magnetic separation and roasting, making the ore processing process more reasonable;
[0025] (2) High-pressure air is used to classify the materials, which can accurately control the classification particle size, ensure the classification quality and the particle size of the roasted materials, and make the suspension roasting system run stably;
[0026] (3) Pre-classification - Another purpose of strong magnetic tailings is to remove low-grade ore powder, reduce the amount of ore fed into the furnace and the amount of processing for subsequent magnetic separation, reduce heat consumption, and prepare feed with suitable particle size and grade for suspension roasting. During the heating process of the suspension roasting furnace, weakly magnetic iron minerals are converted into strongly magnetic iron minerals, which are then magnetically separated to obtain iron ore concentrate products with an iron grade greater than 65%.
[0027] This method can achieve "pre-discarding tailings" of iron ore and obtain high-grade iron concentrate products, achieving the goal of "reducing costs and increasing efficiency". The total iron recovery rate is greater than 90%, the indicators are stable, the economy is good, and the efficient comprehensive utilization of iron ore can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0030] The pre-classification equipment used in the embodiment of the present invention is a pneumatic classifier.
[0031] The crusher used in the embodiment of the present invention is a high pressure roller mill.
[0032] The weak magnetic separator used in the embodiment of the present invention is a permanent magnetic drum magnetic separator.
[0033] The high-intensity magnetic separator used in the embodiment of the present invention is a vertical ring electromagnetic pulsating high-gradient magnetic separator.
[0034] The suspension roasting furnace used in the embodiment of the present invention is a fluidized suspension roasting furnace.
[0035] The process flow chart of the utilization method of iron ore pre-gas classification-strong magnetic tailings discarding-suspension roasting provided by the present invention is as follows: Figure 1 shown.
[0036] Example 1
[0037] The main iron minerals of the iron ore in this embodiment are hematite, limonite and a small amount of magnetite. The raw material TFe grade is 22.51%. A method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting is carried out in the following steps:
[0038] (1) crushing hematite ore (maximum particle size of 12 mm) to a particle size of 4 mm, and performing pneumatic classification on the crushed product to obtain a coarse particle product (particle size > 3 mm) and a fine particle product (particle size ≤ 3 mm); crushing and grinding the coarse particle product to a particle size ≤ 3 mm, and then performing magnetic separation on the ground product, first using a weak magnetic separator to perform weak magnetic separation to obtain a weak magnetic concentrate and a weak magnetic tailing, and controlling the magnetic field strength to 0.2 T, and using a strong magnetic separator to perform strong magnetic separation on the weak magnetic tailing, and controlling the magnetic field strength to 0.6 T, to obtain a strong magnetic concentrate and a strong magnetic tailing, and the weak magnetic concentrate and the strong magnetic concentrate are combined as a mixed coarse concentrate product, and the strong magnetic tailing is discharged as a qualified tailing;
[0039] (2) The fine-grained product is mixed with the powdery mixed coarse concentrate product and then fed into a suspension roasting furnace, gradually heated to 550°C for high-temperature roasting for 2 seconds to remove impurities such as crystal water in the mixed ore, and then placed in a hydrogen-based reducing atmosphere at 500°C for 10 minutes in a suspended state, and then cooled to 200°C in a nitrogen atmosphere under oxygen-free conditions, and then cooled to 50°C by passing air to obtain a roasted ore;
[0040] (3) The roasted ore is passed into water to form a slurry with a weight concentration of 40%, and then magnetic separation is carried out using a permanent magnetic drum magnetic separator with a magnetic force controlled at 0.1 T to obtain a weak magnetic separation concentrate and a segmented weak magnetic separation tailings. The magnetic separation concentrate is used as a qualified iron ore concentrate product, and the weak magnetic separation tailings are used as final tailings.
[0041] (4) The obtained iron concentrate product TFe grade is 65.01%, and the iron recovery rate is 90.63%. The obtained strong magnetic tailings TFe grade is 3.27%, and the iron recovery rate is 4.08%. The obtained weak magnetic tailings TFe grade is 3.49%, and the iron recovery rate is 5.28%.
[0042] Example 2
[0043] The main iron minerals of the iron ore in this embodiment are hematite and limonite. The raw material TFe grade is 25.15%. The method is carried out according to the following steps:
[0044] (1) crushing hematite ore (maximum particle size of 15 mm) to a particle size of 4 mm, and performing pneumatic classification on the crushed product to obtain a coarse particle product (particle size>3 mm) and a fine particle product (particle size≤3 mm); crushing and grinding the coarse particle product to a particle size of ≤3 mm, and then performing magnetic separation on the ground product, firstly using a weak magnetic separator to perform weak magnetic separation to obtain a weak magnetic concentrate and a weak magnetic tailing, and controlling the magnetic field strength to be 0.25 T, and using a strong magnetic separator to perform strong magnetic separation on the weak magnetic tailing, and controlling the magnetic field strength to be 0.55 T, to obtain a strong magnetic concentrate and a strong magnetic tailing, and the weak magnetic concentrate and the strong magnetic concentrate are combined as a mixed coarse concentrate product, and the strong magnetic tailing is discharged as a qualified tailing;
[0045] (2) The fine-grained product is mixed with the powdery mixed coarse concentrate product and then fed into a suspension roasting furnace, gradually heated to 570°C for high-temperature roasting for 5 seconds to remove impurities such as crystal water in the mixed ore, and then placed in a hydrogen-based reducing atmosphere under 540°C suspension state for 15 minutes, and then cooled to 250°C under nitrogen atmosphere protection under oxygen-free conditions, and then cooled to 100°C by passing air to obtain a roasted ore;
[0046] (3) The roasted ore is passed into water to form a slurry with a weight concentration of 50%, and then magnetic separation is carried out using a permanent magnetic drum magnetic separator with a magnetic force controlled at 0.25 T to obtain a weak magnetic separation concentrate and a segmented weak magnetic separation tailings. The magnetic separation concentrate is used as a qualified iron ore concentrate product, and the weak magnetic separation tailings are used as final tailings.
[0047] (4) The obtained iron concentrate product TFe grade is 65.12%, and the iron recovery rate is 91.40%. The obtained strong magnetic tailings TFe grade is 4.50%, and the iron recovery rate is 4.60%. The obtained weak magnetic tailings TFe grade is 3.05%, and the iron recovery rate is 4.00%.
[0048] Example 3
[0049] The main iron minerals of the iron ore in this embodiment are hematite and a small amount of siderite. The raw material TFe grade is 28.35%. The method is carried out according to the following steps:
[0050] (1) crushing hematite ore (maximum particle size of 15 mm) to a particle size of 5 mm, and performing pneumatic classification on the crushed product to obtain a coarse particle product (particle size > 3 mm) and a fine particle product (particle size ≤ 3 mm); crushing and grinding the coarse particle product to a particle size ≤ 3 mm, and then performing magnetic separation on the ground product, firstly using a weak magnetic separator to perform weak magnetic separation to obtain a weak magnetic concentrate and a weak magnetic tailing, and controlling the magnetic field strength to be 0.2 T, and using a strong magnetic separator to perform strong magnetic separation on the weak magnetic tailing, and controlling the magnetic field strength to be 0.5 T, to obtain a strong magnetic concentrate and a strong magnetic tailing, and the weak magnetic concentrate and the strong magnetic concentrate are combined as a mixed coarse concentrate product, and the strong magnetic tailing is discharged as a qualified tailing;
[0051] (2) The fine-grained product is mixed with the powdery mixed coarse concentrate product and then fed into a suspension roasting furnace, gradually heated to 600°C for high-temperature roasting for 8 seconds to remove impurities such as crystal water in the mixed ore, and then placed in a hydrogen-based reducing atmosphere under 520°C suspension state for 20 minutes, and then cooled to 250°C under nitrogen atmosphere protection under oxygen-free conditions, and then cooled to 75°C by passing air to obtain a roasted ore;
[0052] (3) The roasted ore is passed into water to form a slurry with a weight concentration of 60%, and then magnetic separation is carried out using a permanent magnetic drum magnetic separator with a magnetic force controlled at 0.2 T to obtain a weak magnetic separation concentrate and a segmented weak magnetic separation tailings. The magnetic separation concentrate is used as a qualified iron ore concentrate product, and the weak magnetic separation tailings are used as final tailings.
[0053] (4) The obtained iron concentrate product TFe grade is 65.59%, and the iron recovery rate is 90.08%. The obtained strong magnetic tailings TFe grade is 4.79%, and the iron recovery rate is 3.89%. The obtained weak magnetic tailings TFe grade is 4.69%, and the iron recovery rate is 6.03%.
[0054] Example 4
[0055] The main iron minerals of the iron ore in this embodiment are hematite and a small amount of limonite. The raw material TFe grade is 30.03%. The method is carried out according to the following steps:
[0056] (1) crushing hematite ore (maximum particle size of 18 mm) to a particle size of 5 mm, and performing pneumatic classification on the crushed product to obtain a coarse particle product (particle size > 3 mm) and a fine particle product (particle size ≤ 3 mm); crushing and grinding the coarse particle product to a particle size ≤ 3 mm, and then performing magnetic separation on the ground product, first using a weak magnetic separator to perform weak magnetic separation to obtain a weak magnetic concentrate and a weak magnetic tailing, and controlling the magnetic field strength to 0.25 T, and using a strong magnetic separator to perform strong magnetic separation on the weak magnetic tailing, and controlling the magnetic field strength to 0.5 T, to obtain a strong magnetic concentrate and a strong magnetic tailing, and the weak magnetic concentrate and the strong magnetic concentrate are combined as a mixed coarse concentrate product, and the strong magnetic tailing is discharged as a qualified tailing;
[0057] (2) The fine-grained product is mixed with the powdery mixed coarse concentrate product and then fed into a suspension roasting furnace, gradually heated to 580°C for high-temperature roasting for 8 seconds to remove impurities such as crystal water in the mixed ore, and then placed in a hydrogen-based reducing atmosphere at 500°C for 25 minutes in a suspended state, and then cooled to 200°C in a nitrogen atmosphere under oxygen-free conditions, and then cooled to 70°C by passing air to obtain a roasted ore;
[0058] (3) The roasted ore is passed into water to form a slurry with a weight concentration of 65%, and then magnetic separation is carried out using a permanent magnetic drum magnetic separator with a magnetic force controlled at 0.25 T to obtain a weak magnetic separation concentrate and a segmented weak magnetic separation tailings. The magnetic separation concentrate is used as a qualified iron ore concentrate product, and the weak magnetic separation tailings are used as final tailings.
[0059] (4) The obtained iron concentrate product TFe grade is 66.02%, and the iron recovery rate is 90.04%. The obtained strong magnetic tailings TFe grade is 5.50%, and the iron recovery rate is 2.72%. The obtained weak magnetic tailings TFe grade is 5.45%, and the iron recovery rate is 7.24%.
[0060] Example 5
[0061] The main iron minerals of the iron ore in this embodiment are hematite and a small amount of limonite. The raw material TFe grade is 32.22%. The method is carried out according to the following steps:
[0062] (1) crushing hematite ore (maximum particle size of 30 mm) to a particle size of 6 mm, and performing pneumatic classification on the crushed product to obtain a coarse particle product (particle size>3 mm) and a fine particle product (particle size≤3 mm); crushing and grinding the coarse particle product to a particle size of ≤3 mm, and then performing magnetic separation on the ground product, firstly using a weak magnetic separator to perform weak magnetic separation to obtain a weak magnetic concentrate and a weak magnetic tailing, and controlling the magnetic field strength to be 0.3 T, and using a strong magnetic separator to perform strong magnetic separation on the weak magnetic tailing, and controlling the magnetic field strength to be 0.4 T, to obtain a strong magnetic concentrate and a strong magnetic tailing, and the weak magnetic concentrate and the strong magnetic concentrate are combined as a mixed coarse concentrate product, and the strong magnetic tailing is discharged as a qualified tailing;
[0063] (2) The fine-grained product is mixed with the powdery mixed coarse concentrate product and then fed into a suspension roasting furnace, gradually heated to 650°C for high-temperature roasting for 8 seconds to remove impurities such as crystal water in the mixed ore, and then placed in a hydrogen-based reducing atmosphere for 30 minutes in a suspended state at 520°C, and then cooled to 300°C in a nitrogen atmosphere under oxygen-free conditions, and then cooled to 100°C by passing air to obtain a roasted ore;
[0064] (3) The roasted ore is passed into water to form a slurry with a weight concentration of 70%, and then magnetic separation is carried out using a permanent magnetic drum magnetic separator with a magnetic force controlled at 0.35 T to obtain a weak magnetic separation concentrate and a segmented weak magnetic separation tailings. The magnetic separation concentrate is used as a qualified iron ore concentrate product, and the weak magnetic separation tailings are used as final tailings.
[0065] (4) The obtained iron concentrate product TFe grade is 66.01%, and the iron recovery rate is 90.03%. The obtained strong magnetic tailings TFe grade is 5.78%, and the iron recovery rate is 2.36%. The obtained weak magnetic tailings TFe grade is 6.05%, and the iron recovery rate is 7.61%.
[0066] Example 6
[0067] The main iron minerals of the iron ore in this embodiment are hematite and a small amount of limonite. The raw material TFe grade is 34.57%. The method is carried out according to the following steps:
[0068] (1) crushing hematite ore (maximum particle size of 20 mm) to a particle size of 6 mm, and performing pneumatic classification on the crushed product to obtain a coarse particle product (particle size>3 mm) and a fine particle product (particle size≤3 mm); crushing and grinding the coarse particle product to a particle size of ≤3 mm, and then performing magnetic separation on the ground product, first using a weak magnetic separator to perform weak magnetic separation to obtain a weak magnetic concentrate and a weak magnetic tailing, and controlling the magnetic field strength to be 0.3 T, and using a strong magnetic separator to perform strong magnetic separation on the weak magnetic tailing, and controlling the magnetic field strength to be 0.4 T, to obtain a strong magnetic concentrate and a strong magnetic tailing, and the weak magnetic concentrate and the strong magnetic concentrate are combined as a mixed coarse concentrate product, and the strong magnetic tailing is discharged as a qualified tailing;
[0069] (2) The fine-grained product is mixed with the powdery mixed coarse concentrate product and then fed into a suspension roasting furnace, gradually heated to 650°C for high-temperature roasting for 10 seconds to remove impurities such as crystal water in the mixed ore, and then placed in a hydrogen-based reducing atmosphere for 30 minutes in a suspended state at 540°C, and then cooled to 300°C in a nitrogen atmosphere under oxygen-free conditions, and then cooled to 100°C by passing air to obtain a roasted ore;
[0070] (3) The roasted ore is passed into water to form a slurry with a weight concentration of 70%, and then magnetic separation is carried out using a permanent magnetic drum magnetic separator with a magnetic force controlled at 0.4 T to obtain a weak magnetic separation concentrate and a segmented weak magnetic separation tailings. The magnetic separation concentrate is used as a qualified iron ore concentrate product, and the weak magnetic separation tailings are used as final tailings.
[0071] (4) The obtained iron concentrate product TFe grade is 66.50%, and the iron recovery rate is 90.10%. The obtained strong magnetic tailings TFe grade is 6.78%, and the iron recovery rate is 5.14%. The obtained weak magnetic tailings TFe grade is 7.07%, and the iron recovery rate is 4.76%.
Claims
1. A method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting, characterized in that: Follow these steps: (1) crushing the iron ore to a particle size of ≤30 mm and then performing pneumatic classification to obtain a fine-grained product and a coarse-grained product; the particle size of the fine-grained product is ≤3 mm, and the coarse-grained product is crushed-grinded to a particle size of ≤3 mm to obtain a crushed product; the crushed product is subjected to magnetic separation, firstly weak magnetic separation is performed to obtain a weak magnetic separation concentrate and a weak magnetic separation tailing, and then the weak magnetic separation tailing is subjected to strong magnetic separation to obtain a strong magnetic separation concentrate and a strong magnetic separation tailing, and the weak magnetic separation concentrate and the strong magnetic separation concentrate are combined as a coarse concentrate product, and the strong magnetic tailing is a qualified tailing; (2) feeding the mixed ore obtained by mixing the fine-grained product with the coarse concentrate product into a suspension roasting furnace, gradually heating it for high-temperature roasting to remove impurities such as crystal water in the mixed ore, then placing it in a suspended state under a hydrogen-based reducing atmosphere for heat preservation, and then cooling it to 200-300° C. under a nitrogen atmosphere in the absence of oxygen, and then cooling it to 50-100° C. by introducing air to obtain a roasted ore; (3) The roasted ore is passed into water to form a slurry and then subjected to magnetic separation to obtain a weak magnetic separation concentrate and a segment weak magnetic separation tailings, wherein the magnetic separation concentrate is used as an iron ore concentrate product and the weak magnetic separation tailings are used as qualified tailings.
2. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: The iron grade of the iron ore is 20% to 35%, and the particle size is greater than 10 mm.
3. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: In the magnetic separation method described in step (1), the magnetic force range of weak magnetic separation is 0.1-0.3T, and the magnetic force range of strong magnetic separation is 0.4-0.6T.
4. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: The high temperature roasting temperature in step (2) is 550-650° C., and the time is 2-10 seconds; the temperature of the suspension insulation is 500-540° C., and the insulation time is 10-30 minutes.
5. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: The reducing atmosphere in step (2) is a carbon monoxide atmosphere, a hydrogen atmosphere, or a coal gas atmosphere.
6. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: The iron grade of the coarse-grained product strong magnetic separation tailings in step (1) is 3% to 7%.
7. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: The iron grade of the mixed ore in step (2) is 30% to 45%, and the iron grade of the roasted ore is 32% to 47%.
8. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1 is characterized in that: The weight concentration of the slurry in step (3) is 40% to 70%.
9. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1, characterized in that: The magnetic force range of the magnetic separation in step (3) is 0.1 to 0.4 T.
10. The method for utilizing iron ore pre-pneumatic classification-strong magnetic tailings discarding-suspension roasting according to claim 1, characterized in that: The iron ore concentrate product in step (3) has an iron grade of more than 65% and a total iron recovery rate of more than 90%; the iron grade of the weak magnetic separation tailings is 3% to 8%.
Citation Information
Cited By
Method for recovering iron from iron separation tailings and application