Sintered ore with Kuli powder replacing part of FMG mixed powder and preparation method of sintered ore

By using Kuli powder to replace part of FMG mixed powder in sintered ore and adjusting the constituent materials and sintering process parameters, the problems of low yield and reduced productivity of powder ore are solved, and cost reduction and performance improvement are achieved.

CN118910401APending Publication Date: 2024-11-08WUHAN IRON & STEEL GRP ECHENG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410791089.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, low-priced powder ore such as Kuli powder due to high impurity content and low SiO2 content, resulting in low-quality sintered ore yield, reduced productivity, low-temperature reduction powdering index and drum strength of sintered ore, which cannot be effective. Reduce the cost of distribution.

Method used

Use Kuli powder instead of some FMG mixed powder to adjust the proportion of the composition materials of the mixed powder, increase the SiO2 content, and ignite the multi-stage negative pressure during the sintering cooling process by appropriately increasing the sintering temperature and controlling the wet and dry charge density. Enhance liquid phase consolidation and inhibit low-temperature reduction and powdering.

Benefits of technology

While reducing the ore distribution cost, the yield rate, productivity, low-temperature reduction and drum strength of the sintered ore are improved to ensure the stable and forward-speed blast furnace production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses sintered ore with Kuli powder replacing part of FMG mixed powder and a preparation method of the sintered ore, and belongs to the technical field of metallurgical sintered ore. The raw materials of the sintered ore comprise a mixture and sintered return ore; wherein the composition materials of the mixture comprise uniformly mixed mineral powder, a solvent and fuel; the evenly-mixed mineral powder comprises, by mass, 13%-15% of PB powder, 19%-21% of BRBF powder, 2%-8% of FMG mixed powder, 7%-11% of FMG national king powder, 13%-18% of Kuli powder, 2%-4% of domestic fine powder, 6%-8% of direct-supply iron ore concentrate, 1%-3% of Laos powder, 4%-6% of kane powder and 19%-21% of secondary resources. According to the method, the Kuli powder with the Tfe content not lower than 58%, the SiO2 content not lower than 5.5% and the burning loss within 7.5% is selected to replace part of FMG mixed powder, and the ore blending cost is reduced while the quality of the sintered ore is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgical sintered ore, and in particular to a sintered ore in which Cooley powder replaces part of FMG mixed powder and a preparation method thereof. Background Art

[0002] The grade of FMG mixed powder is about 58%, which belongs to limonite, and has average sintering performance. It is an important component of the iron-containing material for sintering ore blending. In order to reduce costs in the steel industry, lower-priced powder ore is often used to replace part of the high-priced FMG mixed powder to reduce costs. However, low-priced iron ore powder often has high impurity content such as S and P, and low TFe and SiO2 content. For example, the use of a large proportion of cooley powder will lead to low sintering ore yield, reduced productivity, too much proportion of finished ore particle size less than 10mm, and deterioration of the sintering ore low-temperature reduction powder index (RDI), drum strength and other performance, which affects the use effect, thereby limiting its application and failing to achieve a truly effective reduction in ore blending costs. Summary of the invention

[0003] In view of the above shortcomings of the prior art, the present invention provides a sintered ore in which part of the FMG mixed powder is replaced by cooley powder and a preparation method thereof. The present invention uses cooley powder to replace the FMG mixed powder, which can ensure the yield and productivity, reduce the proportion of finished ore particles less than 10 mm, improve the quality indicators of the sintered ore such as the low-temperature reduction pulverization index and the drum strength, and ensure the stable and smooth operation of the blast furnace production, while greatly reducing the ore blending cost.

[0004] In order to achieve the above object, the specific technical scheme of the present invention is as follows:

[0005] A sintered ore in which cooley powder replaces part of FMG mixed powder, wherein the raw materials of the sintered ore include mixed material and sintered return ore (sintered ore with a size of ≤5 mm produced by a granulation screening system in sintering process production); wherein the components of the mixed material include mixed ore powder, solvent, and fuel; the components of the mixed ore powder include, by mass percentage, PB powder 13-15%, BRBF powder 19-21%, FMG mixed powder 2-8%, FMG king powder 7-11%, cooley powder 13-18%, domestic fine powder 2-4%, directly supplied iron ore concentrate 6-8%, Laotian powder 1-3%, Ka powder 4-6%, and secondary resources 19-21%.

[0006] Preferably, the amount of the mixed mineral powder added is 81-85.2% of the total weight of the mixture.

[0007] Preferably, the constituent materials of the solvent and their proportions in the total weight of the mixture are: quicklime 5.2-6.6%, limestone 0.5-2.5%, and dolomite 4.5-5.1%.

[0008] Preferably, the constituent materials of the fuel and their proportions in the total weight of the mixture are: coal powder 2.3-2.4%, coke powder 2.3-2.4%.

[0009] Preferably, the amount of the sintered return ore added is 16-18% of the total weight of the mixture.

[0010] Preferably, the composition of the sintered ore includes, by mass percentage, TFe 55.5-56.2%, FeO 8.5-10%, SiO2 5.5-5.9%, CaO 10.5-11.3%, MgO 1.8-2.0%, Al2O3 2.0-2.15%, and S 0.01-0.03%.

[0011] Preferably, the composition of the PB powder includes, by mass percentage, TFe 60 - 62.5%, SiO2 3.5 -4.8%, CaO 0.05 - 0.3%, S ≤ 0.034%, P ≤ 0.095%, Cu ≤ 0.003%, Al2O3 ≤ 2.26%, and a burn loss of 6.1 - 7.1%.

[0012] Preferably, the composition of the BRBF powder includes, by mass percentage, TFe 62-64%, SiO2 4.4-5.4%, CaO 0.1-0.4%, S ≤ 0.029%, P ≤ 0.067%, Cu ≤ 0.007%, Al2O3 ≤ 1.5%, and a burn loss of 2.3-3.3%.

[0013] Preferably, the components of the FMG mixed powder include, by mass percentage, TFe 58 - 60%, SiO2 5.5 -6.1%, CaO 0.05 - 0.5%, S ≤ 0.039%, P ≤ 0.084%, Cu ≤ 0.003%, Al2O3 ≤ 2.85%, and a burn loss of 7.8 - 10.8%.

[0014] Preferably, the FMG king powder comprises, by mass percentage, TFe 57 - 59%, SiO2 5.6 - 6.1%, CaO 0.1 - 0.5%, S ≤ 0.030%, P ≤ 0.081%, Cu ≤ 0.002%, Al2O3 ≤ 1.81%, and a burn loss of 9.6 -10.6%.

[0015] Preferably, the composition of the Cooley powder includes, by mass percentage, TFe 58.4 - 59.4%, SiO2 5.5- 6.1%, CaO 0.05 - 0.3%, S ≤ 0.073%, P ≤ 0.133%, Cu ≤ 0.010%, Al2O3 ≤ 2.22%, and a burn loss of 6.5 - 7.5%.

[0016] Preferably, the composition of the domestic refined powder includes, by mass percentage, TFe 62 - 64%, SiO2 6.8 -7.8%, CaO 0.1 - 0.5%, S ≤ 0.182%, P ≤ 0.032%, Cu ≤ 0.042%, Al2O3 ≤ 1.15%, and loss on burnt 0.9 - 2%.

[0017] Preferably, the composition of the direct-supplied iron ore concentrate includes, by mass percentage, TFe 63 - 65%, SiO2 3.2- 4.2%, CaO 0.5 - 2%, S ≤ 0.599%, P ≤ 0.016%, Cu ≤ 0.015%, Al2O3 ≤ 1.16%, and a loss on burn of 1.2 - 2.2%.

[0018] Preferably, the composition of the Lao powder includes, by mass percentage, TFe 58.4 - 60.4%, SiO2 7.2- 8.2%, CaO 0.5 - 2%, S ≤ 0.284%, P ≤ 0.056%, Cu ≤ 0.030%, Al2O3 ≤ 1.81%, and a burn loss of 1.6 - 2.6%.

[0019] Preferably, the composition of the card powder includes, by mass percentage, TFe 64 - 66%, SiO2 2.2 -3.2%, CaO 0.1 - 0.5%, S ≤ 0.024%, P ≤ 0.072%, Cu ≤ 0.008%, Al2O3 ≤ 1.56%, and a burn loss of 2.5 - 3.5%.

[0020] Preferably, the constituent materials of the secondary resources and their proportions in the mixed ore powder are: ironmaking gas ash 0-1%, iron oxide scale 0-1%, blast furnace return ore 12-14%, lump ore return powder 1-3%, dust removal ash 0-2%, steel slag tailings 0-2%, and steel slag magnetic separation powder 0-1%.

[0021] Preferably, the composition of the ironmaking gas ash includes, by mass percentage, TFe 40.2 - 42.2%, SiO2 6.3 - 7.3%, CaO 4 - 6%, S ≤ 0.132%, P ≤ 0.071%, Cu ≤ 0.008%, Al2O3 ≤ 2.55%, and burnt loss 26.6 - 28.6%.

[0022] Preferably, the composition of the iron oxide scale includes TFe 59.9-61.9%, SiO2 3-4%, CaO 1-2%, S ≤ 0.163%, P ≤ 0.061%, Cu ≤ 0.015%, Al2O3 ≤ 0.71%, and burn loss 0.1-1%.

[0023] Preferably, the composition of the ore returned from the blast furnace includes, by mass percentage, TFe 54.6 - 56.6%, SiO2 5.1 - 6.1%, CaO 10 - 12%, S ≤ 0.023%, P ≤ 0.073%, Cu ≤ 0.007%, Al2O3 ≤ 2.14%, and a burn loss of 0.1 - 1%.

[0024] Preferably, the components of the lump ore return powder include TFe 60.6 - 62.6%, SiO2 3.2 - 4.2%, CaO 0.1 - 0.3%, S ≤ 0.034%, P ≤ 0.095%, Cu ≤ 0.003%, Al2O3 ≤ 2.26%, and burn loss 5.6 - 7.6%.

[0025] Preferably, the components of the dust removal ash include, by mass percentage, TFe 36.5 - 38.5%, SiO2 6.2 - 7.2%, CaO 11 - 13%, S ≤ 0.136%, P ≤ 0.071%, Cu ≤ 0.008%, Al2O3 ≤ 2.38%, and burnt loss 8 - 10%.

[0026] Preferably, the steel slag tailings have a composition, by mass percentage, of TFe 16.6 - 18.6%, SiO2 16.3 - 17.3%, CaO 38 - 40%, S ≤ 0.111%, P ≤ 0.387%, Cu ≤ 0.001%, Al2O3 ≤ 3.23%, and a burn loss of 1-3%.

[0027] Preferably, the composition of the steel slag magnetic separation powder includes, by mass percentage, TFe 42 - 44%, SiO2 12.8- 13.8%, CaO 27 - 29%, S ≤ 0.084%, P ≤ 1.053%, Cu ≤ 0.006%, Al2O3 ≤ 2.43%, and burn loss 1- 3%.

[0028] FMG mixed powder is limonite, which has a relatively stable composition, but has a high burnout, a large shrinkage rate during the sintering process, and a low self-consolidation strength. When the proportion of added is high, the ore inventory is low, the drum strength of the sintered ore is reduced, resulting in a high coal consumption during the sintering process, which seriously affects the quality of the sintered ore and the cost of the sintering process. The present invention reduces the sintering ore blending cost while appropriately increasing SiO2 by selecting Cooley powder with a Tfe content of not less than 58%, SiO2 of not less than 5.5%, and a burnout of less than 7.5%, so that it can react with the gangue components under lower temperatures and less solid fuel consumption conditions to generate more low-melting-point substances, thereby obtaining a sintered ore with appropriate melting point, good reducibility and drum strength.

[0029] The silicon content in the mixed ore powder directly affects the porosity, strength and other physical properties of the sintered ore, and also affects the chemical reaction path during the sintering process, especially the reaction of iron oxides, and determines the chemical composition and purity of the final product. The present invention adjusts the proportion and moisture content of the Cooley powder and FMG mixed powder to make the content of the mixed ore powder reach TFe 58.4-60.4%, SiO2 4.2 - 6.2%, CaO 2.1 - 3.1%, S ≤ 0.090%, P ≤ 0.1%, Cu ≤ 0.008%, Al2O3 ≤ 1.905%, and the burn loss reaches 4.2 - 5.2%. Further, by stabilizing the moisture content of the mixed ore powder, controlling its average particle size, and controlling the SiO2 content, the quality of the sintered ore is improved, energy consumption is reduced, and thus the production cost is reduced and the production efficiency is improved.

[0030] The size and fluctuation of basicity are affected by the content of CaO, MgO, SiO2, and Al2O3, and the amount of CaO, MgO, SiO2, and Al2O3 is mainly determined by the amount of flux added, and suitable flux can strengthen sintering and is indispensable. Therefore, the flux selected in the present invention is 5.2-6.6% quicklime, 0.5-2.5% limestone, and 4.5-5.1% dolomite.

[0031] Preferably, the limestone contains CaO ≥ 54%, SiO2 ≤ 1.5%, MgO ≥ 0.5%, S ≤ 0.06%, and H2O ≤ 5.0%; particle size: ≤ 3.0 mm (> 3 mm does not exceed 10%).

[0032] Preferably, the quicklime has a content of CaO ≥ 83%, SiO2 ≤ 3.0%, MgO ≤ 7.0%, and S ≤ 0.15%; activity (4mol / L40 ± 1°C, 10min) ≥ 220; particle size: ≤ 3mm (the proportion of >3mm does not exceed 10%).

[0033] Preferably, the dolomite has a composition content of MgO ≥ 19.0%, SiO2 ≤ 3.5%, P ≤ 0.080%, S ≤ 0.040%, and H2O ≤ 5.0%; particle size: ≤ 3.0 mm (the proportion of >3 mm does not exceed 10%).

[0034] Preferably, the proportion of the coke powder having a particle size less than 3 mm is 67-77%.

[0035] Preferably, the proportion of coal powder with a particle size less than 3 mm is 63-73%.

[0036] The method for preparing the sintered ore in which the Cooley powder replaces part of the FMG mixed powder comprises the following steps:

[0037] S1. Batching: Mix the raw materials such as ore powder, solvent, fuel and sintering return ore according to the proportion; the proportion and composition of each raw material have an important influence on the final sinter quality; dolomite and limestone are transported to the batching tank by belt conveyor, and quicklime is directly delivered to the batching tank by sealed tank truck;

[0038] S2. Mixing and granulation: The prepared raw materials are mixed with water to make the water content of the sintered material 6.6%-7.2%, and then granulated by a pelletizer; wherein, 80-90% of the total water is added to the first mixing, the water addition rate is 13-15t / h, and the remaining water is added to the second mixing, and the water addition rate is 2-3t / h; the granulation time is 4-6 minutes;

[0039] S3. Distribution and ignition: 10 - 20mm sintered ore is used as the base material, with a thickness of 70 - 80mm. The round roller feeder and nine-roller distributor are used to evenly distribute the material on the trolley with the base material. The particle size of the raw material is segregated from top to bottom and gradually increases. The granulated sintered material is placed on the sintering equipment and ignited. Pure coke oven gas is used for ignition, and the calorific value of the gas is 9211 kJ / m 3 , the ignition temperature is 1050-1200℃; in order to reduce the negative impact on the quality of sintered ore caused by the sharp drop in the surface sintered ore temperature, the ignition time is 1-2min; the insulation time is 1-2min;

[0040] S4. Sintering: After ignition, the sintering material begins the sintering process, which is accompanied by ventilation treatment, so that the sintering negative pressure is 17-19kPa; during the sintering process, the powder ore particles in the material are bonded to form a block structure;

[0041] S5. Cooling: After sintering, the ore blocks need to be cooled to below 120°C for subsequent processing and use.

[0042] S6. Screening: Three vibrating screens are used to screen the cooled sintered particles. The under-screen material is used as sintering return ore, and the over-screen material is used as sintered ore product.

[0043] Preferably, the sintering machine used in the sintering process is a 260m² belt-type exhaust sintering machine.

[0044] Preferably, the basicity of the sintered ore in the sintering process is controlled to be 1.91 - 1.95.

[0045] Preferably, the proportion of the sintered ore with a particle size less than 10 mm after screening is less than 20%.

[0046] The present invention increases the amount of liquid phase generated during the sintering process by increasing the sintering temperature and the thickness of the material, controlling the relatively low density of wet and dry charge, multi-stage negative pressure during the ignition sintering cooling process, vertical burning speed, etc., so that the liquid phase is fully solidified and the low-temperature reduction pulverization of the sintered ore is inhibited, which is beneficial to further improve the final sintering yield and the sintered ore drum strength index, improve the low-temperature reduction pulverization index of the sintered ore, and further improve the productivity.

[0047] Compared with the prior art, the present invention is beneficial in that:

[0048] (1) The present invention reduces production costs by using Cooley powder to partially replace part of the FMG mixed powder;

[0049] (2) The present invention adopts up to 13-18% of Cooley powder to replace part of the FMG mixed powder, and mixes it with 7-11% FMG king powder and other components in proportion. Only 2-8% of FMG mixed powder is needed for ore blending. The low-temperature reduction pulverization index +3.15 of the obtained sintered ore reaches more than 70%, the drum index reaches more than 77%, and the proportion of the sintered ore with a particle size of less than 10 mm is controlled to less than 20%, thereby improving the quality of the sintered ore and facilitating the stable and smooth operation of the blast furnace smelting process. DETAILED DESCRIPTION

[0050] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] The present invention provides a sintered ore in which part of the FMG mixed powder is replaced by coolie powder. The raw materials of the sintered ore include mixed material and sintered return ore (sintered ore with a size of ≤5 mm produced by the granulation screening system in the sintering process); wherein the components of the mixed material include mixed ore powder, solvent, and fuel; the components of the mixed ore powder include PB powder 13-15%, BRBF powder 19-21%, FMG mixed powder 2-8%, FMG King powder 7-11%, coolie powder 13-18%, domestic fine powder 2-4%, direct iron concentrate 6-8%, Lao powder 1-3%, card powder 4-6%, and secondary resources 19-21%. The composition of the ore powder used in the following examples is shown in Table 1.

[0052] Table 1: Chemical composition of mineral powder used in the examples

[0053]

[0054] Example 1

[0055] The specific preparation steps of the sintered ore in which the Cooley powder replaces the FMG mixed powder in this embodiment are as follows:

[0056] S1. Ingredients: The proportion of mixed ore powder is: PB powder 14.2%, BRBF powder 20.3%, FMG mixed powder 7.5%, FMG king powder 7.4%, domestic fine powder 3.0%, Cooley powder 13.4%, ironmaking gas ash 0.6%, iron oxide scale 0.8%, blast furnace return ore 13.6%, lump ore return powder 2.3%, dust removal ash 1.0%, direct iron ore concentrate 7.1%, Laotian powder 2.0%, card powder 5.1%, steel slag tailings 1.0%, steel slag magnetic separation powder 0.7%; the fuel is 2.35% of the total weight of the mixture and 2.35% of coke powder; the flux is 5.2% of the total weight of the mixture, 2.5% of limestone and 5% of dolomite; the internal return ore is 18% of the total weight of the mixture;

[0057] S2. Mixing and granulation: The prepared raw materials were mixed with water to make the water content of the sintered material 6.9%, and then granulated by a pelletizer; wherein, a mixed addition of 85% of the total water addition amount, the water addition rate was 14t / h, and the second mixed addition of the remaining water, the water addition rate was 2.5t / h; the granulation time was 5 minutes;

[0058] S3. Distribution and ignition: First, select 10-20mm sintered ore as the base material, and spread it 70-80mm thick. Then use the round roller feeder and the nine-roller distributor to evenly distribute the material on the trolley with the base material. The particle size of the raw material segregates from top to bottom and gradually increases. The granulated sintered material is placed on the sintering equipment and ignited. Pure coke oven gas is used for ignition, and the calorific value of the gas is 9211 kJ / m 3 ; The ignition temperature is 1075℃; In order to reduce the negative impact on the quality of sintered ore caused by the sharp drop in the surface sintered ore temperature, the ignition time is 1min; the holding time is 2min;

[0059] S4. Sintering: After ignition, the sintering material begins the sintering process, which is accompanied by ventilation treatment, so that the sintering negative pressure is 18.5kPa; during the sintering process, the powder ore particles in the material are bonded to form a block structure;

[0060] S5. Cooling: Cooling the sintered ore to 100°C;

[0061] S6. Screening: Three vibrating screens are used to screen the cooled sintered particles. The under-screen material is used as sintering return ore, and the over-screen material is used as sintered ore product.

[0062] Example 2

[0063] The specific preparation steps of the sintered ore in which the cooley powder replaces the FMG mixed powder in this embodiment are basically the same as those in Example 1, except that, step S1. Ingredients: The proportions of the mixed ore powders are: 14.2% PB powder, 20.3% BRBF powder, 3.2% FMG mixed powder, 10.1% FMG king powder, 3.0% domestic fine powder, 15% cooley powder, 0.6% ironmaking gas ash, 0.8% iron oxide scale, 13.6% return ore from outside the blast furnace, 2.3% lump ore return powder, 1.0% dust removal ash, 7.1% directly supplied iron ore, 2.0% Laotian powder ore, 5.1% stuck powder, 1.0% steel slag tailings, and 0.7% steel slag magnetic separation powder; the fuel is 2.35% of coal powder and 2.35% of coke powder of the total weight of the mixture; the flux is 5.4% of quicklime, 2.5% of limestone and 5.1% of dolomite of the total weight of the mixture; the internal return ore is 17% of the total weight of the mixture.

[0064] Example 3

[0065] The specific preparation steps of the sintered ore in which the cooley powder replaces the FMG mixed powder in this embodiment are basically the same as those in Example 1, except that, step S1. Ingredients: The proportions of the mixed ore powders are: 14.2% PB powder, 20.3% BRBF powder, 3.0% FMG mixed powder, 9.1% FMG king powder, 3.0% domestic fine powder, 16.2% cooley powder, 0.6% ironmaking gas ash, 0.8% iron oxide scale, 13.6% return ore from outside the blast furnace, 2.3% lump ore return powder, 1.0% dust removal ash, 7.1% directly supplied iron ore concentrate, 2.0% Laotian powder ore, 5.1% stuck powder, 1.0% steel slag tailings, and 0.7% steel slag magnetic separation powder; the fuel is 2.4% of coal powder and 2.4% of coke powder of the total weight of the mixture; the flux is 5.2% of quicklime, 2.5% of limestone and 5% of dolomite of the total weight of the mixture; the internal return ore is 18% of the total weight of the mixture.

[0066] Example 4

[0067] The specific preparation steps of the sintered ore in which the cooley powder replaces the FMG mixed powder in this embodiment are basically the same as those in Example 1, except that, step S1. Ingredients: The proportions of the mixed ore powders are: 14.2% PB powder, 20.3% BRBF powder, 3.0% FMG mixed powder, 9.1% FMG king powder, 3.0% domestic fine powder, 16.2% cooley powder, 0.6% ironmaking gas ash, 0.8% iron oxide scale, 13.6% return ore from outside the blast furnace, 2.3% lump ore return powder, 1.0% dust removal ash, 7.1% directly supplied iron ore concentrate, 2.0% Laotian powder ore, 5.1% stuck powder, 1.0% steel slag tailings, and 0.7% steel slag magnetic separation powder; the fuel is 2.35% of coal powder and 2.35% of coke powder of the total weight of the mixture; the flux is 6.5% of quicklime, 0.5% of limestone and 4.5% of dolomite of the total weight of the mixture; the internal return ore is 18% of the total weight of the mixture.

[0068] Example 5

[0069] The specific preparation steps of the sintered ore in which the cooley powder replaces the FMG mixed powder in this embodiment are basically the same as those in Example 1, except that, step S1. Ingredients: The proportions of the mixed ore powders are: 14.2% PB powder, 20.3% BRBF powder, 3.0% FMG mixed powder, 9.1% FMG king powder, 3.0% domestic fine powder, 16.2% cooley powder, 0.6% ironmaking gas ash, 0.8% iron oxide scale, 13.6% return ore from outside the blast furnace, 2.3% lump ore return powder, 1.0% dust removal ash, 7.1% directly supplied iron ore concentrate, 2.0% Laotian powder ore, 5.1% stuck powder, 1.0% steel slag tailings, and 0.7% steel slag magnetic separation powder; the fuel is 2.35% of coal powder and 2.35% of coke powder of the total weight of the mixture; the flux is 5.2% of quicklime, 2.5% of limestone and 4.5% of dolomite of the total weight of the mixture; the internal return ore is 18% of the total weight of the mixture.

[0070] Example 6

[0071] The specific preparation steps of the sintered ore in which the cooley powder replaces the FMG mixed powder in this embodiment are basically the same as those in Example 1, except that, step S1. Ingredients: The proportions of the mixed ore powders are: 14.2% PB powder, 20.3% BRBF powder, 3.1% FMG mixed powder, 8.1% FMG king powder, 3.0% domestic fine powder, 17.1% cooley powder, 0.6% ironmaking gas ash, 0.8% iron oxide scale, 13.6% return ore from outside the blast furnace, 2.3% lump ore return powder, 1.0% dust removal ash, 7.1% directly supplied iron ore concentrate, 2.0% Laotian powder ore, 5.1% stuck powder, 1.0% steel slag tailings, and 0.7% steel slag magnetic separation powder; the fuel is 2.3% of coal powder and 2.3% of coke powder of the total weight of the mixture; the flux is 5.2% of quicklime, 2% of limestone and 4.5% of dolomite of the total weight of the mixture; the internal return ore is 18% of the total weight of the mixture.

[0072] Comparative Examples 1-6

[0073] The preparation steps of the sintered ore in this comparative example are basically the same as those in Example 1, except that the proportion of the mixed ore powder is different, see Table 2 for details.

[0074] Table 2: Proportions of mixed ore powders of Examples 1-6 and Comparative Examples 1-6 (%)

[0075]

[0076] Table 3: Sintered ore raw material ratios of Examples 1-6 (%)

[0077]

[0078] Table 4: Chemical composition of sintered ore of Examples 1-6 and Comparative Examples 1-6 (%)

[0079]

[0080] Table 5: Sintered ore quality of Examples 1-6 and Comparative Examples 3-6

[0081]

[0082] The purchase price of FMG mixed powder is about 794.24 yuan / ton, the purchase price of FMG king powder is about 786.63 yuan / ton, and the purchase price of Australian coolie powder is about 769.75 yuan / ton. It can be seen from Table 5 that the sintered ore prepared in Examples 1-6 has a low-temperature reduction pulverization index +3.15 of more than 70%, a drum index of more than 77%, and a sintered ore particle size of less than 10 mm. The proportion is less than 20%, which can meet the requirements of most blast furnace production and use. It shows that replacing FMG mixed powder with part of coolie powder can reduce the cost of ore blending while ensuring the quality of the sintered ore. If all the coolie powder in Example 1 is replaced with FMG mixed powder, the quality of the sintered ore is basically the same as that of Example 1, but the cost of ore blending is 1.1 yuan / ton higher than that of Example 1. If the amount of Cooley powder added is too large (Comparative Example 1), the total iron (TFe) content of the sintered ore will be lower than 55%, and the S content will be too high, which will lead to a decrease in the quality of the sintered ore and an increase in the ironmaking cost. Compared with Example 1, the difference between Comparative Example 2 and Example 1 is that the amount of PB powder (TFe content of 61.61%) is increased by 5%, while the amount of BRBF powder (TFe content of 63.12%) is reduced by 5%, resulting in the TFe content of the sintered ore in Comparative Example 2 being lower than 55%, which will lead to a decrease in the quality of the sintered ore and an increase in the ironmaking cost.

[0083] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. A sintered ore in which Cooley powder replaces part of the FMG mixed powder. It is characterized in that The raw materials of the sintered ore include a mixture and sintered return ore; wherein the components of the mixture include mixed ore powder, solvent, and fuel; the components of the mixed ore powder include, by mass percentage, PB powder 13-15%, BRBF powder 19-21%, FMG mixed powder 2-8%, FMG King powder 7-11%, Cooley powder 13-18%, domestic fine powder 2-4%, directly supplied iron ore concentrate 6-8%, Laotian powder 1-3%, Ka powder 4-6%, and secondary resources 19-21%.

2. The sintered ore in which the Cooley powder replaces part of the FMG mixed powder according to claim 1, It is characterized in that The amount of the mixed mineral powder added is 81-85.2% of the total weight of the mixture.

3. The sintered ore in which the Cooley powder according to claim 1 replaces part of the FMG mixed powder, It is characterized in that The constituent materials of the solvent and their proportions in the total weight of the mixed material are: quicklime 5.2-6.6%, limestone 0.5-2.5%, and dolomite 4.5-5.1%.

4. The sintered ore in which the Cooley powder replaces part of the FMG mixed powder according to claim 1, It is characterized in that The constituent materials of the fuel and their proportions in the total weight of the mixture are: coal powder 2.3-2.4%, coke powder 2.3-2.4%.

5. The sintered ore in which the Cooley powder replaces part of the FMG mixed powder according to claim 1, It is characterized in that The amount of the sintered ore added is 16-18% of the total weight of the mixture.

6. The sintered ore in which the Cooley powder replaces part of the FMG mixed powder according to claim 1, It is characterized in that The constituent materials of the secondary resources and their proportions in the mixed ore powder are: ironmaking gas ash 0-1%, iron oxide scale 0-1%, blast furnace return ore 12-14%, lump ore return powder 1-3%, dust removal ash 0-2%, steel slag tailings 0-2%, and steel slag magnetic separation powder 0-1%.

7. The sintered ore in which the Cooley powder replaces part of the FMG mixed powder according to claim 1, It is characterized in that The composition of the sintered ore includes TFe 55.5-56.2%, FeO 8.5-10%, SiO 2 5.5 -5.9%, CaO 10.5 - 11.3%, MgO 1.8 - 2.0%, Al 2 O 3 2.0 - 2.15%, S 0.01 - 0.03%.

8. A method for preparing sintered ore in which part of the FMG mixed powder is replaced by cooley powder as claimed in any one of claims 1 to 7, It is characterized in that The steps include: S1. Batching: Batching the raw materials of sintered ore according to the proportion; S2 mixing granulation: the above prepared raw materials are mixed with water and then granulated; S3. Material laying and ignition: Use 10 - 20mm sintered ore as the base material, lay 70 - 80mm thick, then lay and ignite; S4. Sintering: After ignition, the sintering material begins the sintering process, and the sintering process is accompanied by exhaust treatment, so that the sintering negative pressure is 17-19 kPa; S5. Cooling: Cool the sintered ore to below 120°C; S6. Screening: The cooled sintered particles are screened and the screened particles are used as sintered ore products.

9. The method for preparing sintered ore in which cooley powder replaces part of FMG mixed powder according to claim 8, It is characterized in that The basicity of the sintered ore in the sintering process is 1.91 - 1.

95.