Preparation process of oxidized pellets
By accurately controlling the preheating and roasting process conditions of oxidized pellets, the problem of uncertain compressive strength of oxidized pellets is solved, and efficient resource utilization and solid waste reduction are achieved.
Patent Information
- Application Number
- CN202410924040.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
The existing oxidized pellet preparation process cannot accurately adjust the process conditions, resulting in uncertain compressive strength, resulting in waste of resources and increased solid waste.
By controlling the temperature of the preheating device, the residence time of the oxidized pellet materials in the preheating device and the oxygen content in the preheating device, the compressive strength of the preheating pellet is accurately adjusted; at the same time, the temperature of the calcining device and the oxidized pellet are controlled and the temperature of the calcining device and the oxidized pellet are controlled. The calcination time of the ball in the roasting device ensures the compressive strength of the oxidized roasted pellets.
Accurate compressive strength control of oxidized pellets is achieved, breakage in iron smelting or steelmaking processes is avoided, solid waste generation is reduced, and process efficiency and resource utilization are improved.
Smart Images

Figure CN118910402A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to oxidation pellet production technology, and in particular to a preparation process for ensuring the compressive strength of oxidation pellets through precise control, belonging to the technical field of oxidation pellet production. Background Art
[0002] Oxidation pelletization is one of the important methods for powder ore agglomeration. First, the powder ore is added with appropriate amount of water, binder and / or fuel to form green balls with uniform viscosity and sufficient strength. After drying and preheating, they are roasted in an oxidizing atmosphere to make the green balls agglomerate and form pellets. This method is particularly suitable for processing fine concentrate powder. Pellets have good cold strength, reducibility and particle size composition. In the steel industry, pellets and sintered ore are also important blast furnace materials.
[0003] Compared with sintered ore, pelletized ore is a higher quality raw material for blast furnace ironmaking, with the advantages of high iron grade, good metallurgical properties, low process energy consumption and pollutant emissions. In recent years, with the development of the steel industry, the domestic production of pelletized ore has shown a gradual upward trend, and a number of large-scale chain grate machine-rotary kiln and belt roaster pelletizing projects have been newly built.
[0004] In the existing oxidation pelletization process, chain grate-rotary kiln system, belt roasting machine system and vertical furnace system are usually used to prepare oxidation pellets. Regardless of the equipment system used for the treatment of oxidation pellets, the oxidation pellet materials must go through the stages of preheating and oxidation roasting. Oxidation roasting pellets are used in blast furnace production and are directly added to the blast furnace as raw materials. The blast furnace has high requirements for the air permeability of the raw materials. The materials added to the blast furnace must have a certain compressive strength to avoid the materials from bursting in the blast furnace, otherwise a large amount of slag will be produced, increasing the subsequent treatment amount of solid waste. At the same time, the oxidation roasting pellets need to go through a cooling process after oxidation roasting. The oxidation pellets themselves must exist in the preheating device, oxidation roasting device and cooling device for a period of time. At the same time, they inevitably move (or roll) between devices or different positions of the system. Oxidation pellets with low compressive strength are very easy to break. The broken oxidation pellets cannot be used in subsequent processes, resulting in waste of resources and increase of solid waste. Therefore, compressive strength is the core indicator of oxidative roasting pellets, and preparing oxidative roasting pellets with specified compressive strength is a necessary condition for the oxidative pellet preparation process.
[0005] In the prior art, the preparation process of oxidized pellets is set according to the experience of workers, and the quality of the oxidized roasted pellets is adjusted by feedback. Through continuous trials, different process conditions are adjusted so that the compressive strength of the oxidized roasted pellets can meet the requirements for the oxidized pellets to enter the blast furnace. The means in the prior art, first of all, the adjustment target is not clear, and it is necessary to continuously try different process conditions, which brings great uncertainty to the preparation process; secondly, the adjustment amount is not clear, and the adjustment is made for different process conditions. The adjustment range of the process conditions needs to be continuously tried. After debugging, it takes a cycle to determine whether it meets the requirements, which greatly delays the preparation of oxidized pellets; at the same time, the adjustment range is prone to be too large or too small, and precise adjustment and control cannot be achieved, resulting in a waste of resources. Summary of the invention
[0006] In view of the technical problem that the oxidized pellet preparation process in the prior art cannot be accurately adjusted and cannot achieve the guarantee of the compressive strength of the oxidized pellets by accurately controlling the process conditions, the present invention proposes a preparation process for oxidized pellets, which controls the temperature in the preheating device, the residence time of the oxidized pellet material in the preheating device, and the oxygen content in the gas in the preheating device, thereby ensuring the compressive strength of the oxidized pellets after the oxidized pellet material is preheated; and controls the temperature in the roasting device and the roasting time of the oxidized pellets in the roasting device, thereby ensuring the compressive strength of the oxidized roasted pellets after the oxidized pellets are roasted. The present invention accurately controls the process conditions of the oxidized pellets in the preheating and oxidizing roasting processes, ensures the strength of the pre-oxidized pellets after preheating and the compressive strength of the oxidized pellets obtained after the oxidizing roasting process, thereby ensuring the subsequent process raw material performance of the oxidized pellets, avoiding the rupture of the oxidized pellets in the ironmaking or steelmaking process, and reducing the generation of solid waste.
[0007] According to a first embodiment provided by the present invention, a process for preparing oxidized pellets is provided.
[0008] A process for preparing oxidized pellets, the process comprising the following steps: (1) Batching: The raw materials for oxidation pellets are mixed and pelletized to obtain oxidation pellet materials; (2) Preheating: The oxidized pellet material is transported to the preheating device, and the oxidized pellet material is preheated to obtain preoxidized pellets; wherein: the temperature in the preheating device, the residence time of the oxidized pellet material in the preheating device, and the oxygen content in the gas in the preheating device are controlled, so as to ensure the compressive strength of the preoxidized pellets after the oxidized pellet material passes through the preheating device; (3) Calcination: The pre-oxidized pellets are transported to a calcination device, and the pre-oxidized pellets are subjected to oxidative calcination to obtain oxidatively calcined pellets; wherein: the temperature in the calcination device and the calcination time of the pre-oxidized pellets in the calcination device are controlled, thereby ensuring the compressive strength of the oxidatively calcined pellets after the pre-oxidized pellets are calcined.
[0009] In the present invention, the control of step (2) is specifically as follows: Y1=a*(0.000005*T1 4 - 0.0195*T1 3 + 26.91*T1 2 - 16453.06*T1+ 3757787.50) + b*(1.2308*t1 3 - 45.53*t1 2 + 575.16*t1- 1135.10) + c*(0.2671*C1 4 - 23.0660*C1 3 +736.06*C1 2 - 10211*C1+ 52534); Where: Y1 is the compressive strength of pre-oxidized pellets, N·P -1 ; T1 is the temperature in the preheating device, ℃; t1 is the residence time of the oxidized pellet material in the preheating device, h; C1 is the volume percentage of oxygen in the gas in the preheating device, %; a is the preheating process temperature adjustment coefficient; b is the preheating process residence time adjustment coefficient; c is the preheating process oxygen content adjustment coefficient; a+b+c=1.
[0010] In the present invention, the control of step (3) is specifically as follows: Y2=d*(0.00007*T2 3 - 0.2315*T2 2 + 249.12*T2- 91120.18) + e*(0.4640*t2 3 -27.0708*t2 2 + 524.20*t2- 495.10); Where: Y2 is the compressive strength of the oxidatively roasted pellets, N·P -1 ; T2 is the temperature in the roasting device, ℃; t2 is the roasting time of the oxidized pellets in the roasting device, h; d is the roasting process temperature adjustment coefficient; e is the roasting time adjustment coefficient; d+e=1.
[0011] In the present invention, the adjustment coefficient is a>b>c.
[0012] Preferably, the value of a is 0.4-0.5, the value of b is 0.3-0.35, and the value of c is 0.15-0.3.
[0013] In the present invention, the adjustment coefficient d>e.
[0014] Preferably, the value of d is 0.55-0.65, and the value of e is 0.35-0.45.
[0015] Preferably, the preparation of the oxidized pellets adopts a chain grate and a rotary kiln system. The preheating device is a chain grate, and the preheating in step (2) is completed in the chain grate. The roasting device is a rotary kiln, and the roasting in step (3) is completed in the rotary kiln.
[0016] Preferably, the preparation of the oxidized pellets is completed by a belt roaster. The belt roaster includes a preheating section and a roasting section. The preheating device is the preheating section of the belt roaster, and the preheating in step (2) is completed in the preheating section of the belt roaster. The roasting device is the roasting section of the belt roaster, and the roasting in step (3) is completed in the roasting section of the belt roaster.
[0017] Preferably, the preparation of the oxidized pellets is completed in a vertical furnace. The vertical furnace includes a preheating section and a roasting section. The preheating device is the preheating section of the vertical furnace, and the preheating in step (2) is completed in the preheating section of the vertical furnace. The roasting device is the roasting section of the vertical furnace, and the roasting in step (3) is completed in the roasting section of the vertical furnace.
[0018] Preferably, the vertical furnace is a vertical electric furnace.
[0019] Preferably, the vertical electric furnace is heated by microwaves.
[0020] In the present invention, the compressive strength of the pre-oxidized pellets is not less than 500 N·P -1 , preferably not less than 600 N·P -1 , more preferably not less than 800 N·P -1 .
[0021] In the present invention, the compressive strength of the oxidatively roasted pellets is not less than 2300 N·P -1 , preferably not less than 2400 N·P -1 , more preferably not less than 2500 N·P -1 .
[0022] In the present invention, the raw material for oxidized pellets is an iron-containing material; optionally, it also includes one or more of a fuel, a binder, and water.
[0023] In the present invention, the raw materials of the oxidized pellets are the same as the conventional raw materials in the prior art, and the system or device for preparing the oxidized pellets also adopts the prior art. However, according to the compressive strength requirements of the oxidized pellets, the process conditions of the preheating process and the roasting process in the oxidized pellet preparation process are precisely controlled to ensure the compressive strength of the oxidized pellets.
[0024] The raw materials and preparation systems of oxidized pellets have mature existing technologies, and the preparation of oxidized pellets must go through preheating and roasting processes. Through research and experiments, the inventors have obtained the process conditions that affect the compressive strength of pre-oxidized pellets after the preheating process in the preparation process of oxidized pellets; through research and experiments, the inventors have obtained the process conditions that affect the compressive strength of oxidized roasted pellets after the oxidized roasting process in the preparation process of oxidized pellets. Through the exploration of the process, the process conditions that affect the compressive strength are obtained, and the correlation between each process condition and the compressive strength is obtained. Through the relationship between compressive strength and process conditions, the compressive strength of the oxidized pellets can be ensured by accurately controlling the process conditions of the preheating process and the roasting process. It is also possible to reasonably adjust one or more process conditions according to the actual process of oxidized pellet preparation through the correlation relationship, thereby ensuring the compressive strength of the oxidized pellets.
[0025] When the inventor explored the process conditions that affect the compressive strength of oxidized pellets in the preheating process, it was concluded through experiments that the preheating temperature, preheating time and oxygen content in the gas in the preheating section directly affect the compressive strength of the pre-oxidized pellets, and these three process conditions have the greatest impact, and the impact of other process conditions on the compressive strength can be ignored.
[0026] Under the premise that the process parameters for preparing oxidized pellets are stable, the relationship between the preheating temperature T1, preheating time t1, oxygen content C1 in the gas and the quality Y (compressive strength) of the oxidized pellets is established.
[0027] First, while ensuring that the preheating time and the oxygen content in the gas in the preheating section remain unchanged, the preheating temperature T1 in the preheating section is adjusted, and the compressive strength of the preoxidized pellets after the oxidized pellets are tested at different preheating temperatures. The compressive strength of the preoxidized pellets is obtained at different preheating temperatures T1 in the preheating section, and the relationship curve between the compressive strength and the preheating temperature T1 in the preheating section is plotted as shown in the figure. Figure 1 As shown, according to the curve fitting, the relationship between the compressive strength and the preheating temperature T1 in the preheating section is: Y1=f(T1)= 0.000005*T1 4 - 0.0195*T1 3 + 26.91*T1 2 - 16453.06*T1+ 3757787.50.
[0028] The second step is to ensure that the preheating temperature and the oxygen content in the gas in the preheating section remain unchanged, adjust the residence time t1 of the oxidized pellet material in the preheating section, detect the compressive strength of the preoxidized pellets after different residence times, obtain the compressive strength of the preoxidized pellets at different residence times t1 of the oxidized pellet material in the preheating section, and draw a relationship curve between the compressive strength and the residence time t1 of the oxidized pellet material in the preheating section, as shown in FIG. Figure 2 As shown, according to the curve fitting, the relationship between the compressive strength and the residence time t1 of the oxidized pellet material in the preheating section is: Y1=f(t1)= 1.2308*t1 3 - 45.53*t1 2 + 575.16*t1- 1135.10.
[0029] The third step is to ensure that the preheating temperature in the preheating section and the residence time of the oxidized pellet material in the preheating section remain unchanged, adjust the oxygen content C1 in the gas in the preheating device, detect the compressive strength of the oxidized pellets after the oxidized pellet material passes through the preheating device with different oxygen contents, obtain the compressive strength of the oxidized pellets under different oxygen contents C1 in the preheating device, and draw a relationship curve between the compressive strength and the oxygen content C1 in the preheating device, as shown in FIG. Figure 3 As shown, according to the curve fitting, the relationship between the compressive strength and the oxygen content C1 in the preheating device is: Y1=f(C1)=0.2671*C1 4 - 23.0660*C1 3 + 736.06*C1 2 - 10211*C1+ 52534.
[0030] The fourth step is to test the influence of each process condition on the compressive strength according to the three process conditions that affect the compressive strength of the pre-oxidized pellets, set the influence factor of the process condition on the compressive strength and verify the accuracy, and obtain the preheating process temperature adjustment coefficient, preheating process residence time adjustment coefficient, and preheating process oxygen content adjustment coefficient. The process conditions that affect the compressive strength of the oxidized pellets in the entire preheating process are as follows: Y1=a*(0.000005*T1 4 - 0.0195*T1 3 + 26.91*T1 2 - 16453.06*T1+ 3757787.50) + b*(1.2308*t1 3 - 45.53*t1 2 + 575.16*t1- 1135.10) + c*(0.2671*C1 4 - 23.0660*C1 3 +736.06*C1 2 - 10211*C1+ 52534); Where: Y1 is the compressive strength of pre-oxidized pellets, N·P -1; T1 is the temperature in the preheating device, ℃; t1 is the residence time of the oxidized pellet material in the preheating device, h; C1 is the volume percentage of oxygen in the gas in the preheating device, %; a is the preheating process temperature adjustment coefficient; b is the preheating process residence time adjustment coefficient; c is the preheating process oxygen content adjustment coefficient; a+b+c=1.
[0031] When the inventors explored the process conditions affecting the compressive strength of pre-oxidized pellets in the oxidation roasting process, they ensured that the compressive strength of the pre-oxidized pellets met the basic conditions (greater than 500 N·P -1 ) under the condition of oxidative roasting, the influence of the roasting process on the compressive strength of the oxidative roasted pellets was studied. Since the oxidative roasting process is an oxidative condition, which is a necessary condition for the preparation of oxidative pellets, there is sufficient oxygen in the oxidative roasting process. Through the test, it was found that the temperature in the roasting device and the roasting time of the oxidative pellets in the roasting device directly affect the compressive strength of the oxidative roasted pellets, and these two process conditions have the greatest influence, and the influence of other process conditions on the compressive strength can be ignored.
[0032] Under the premise of stable process parameters of pre-oxidized pellet preparation, the compressive strength of the prepared pre-oxidized pellets is guaranteed to be greater than 500 N·P -1 Then, the relationship between the roasting temperature T2, roasting time t2 and the mass Y2 (compressive strength) of the roasted pellets in the oxidation roasting stage is established.
[0033] First, while ensuring that the roasting time in the roasting section remains unchanged, the roasting temperature T2 in the oxidation roasting section is adjusted, and the compressive strength of the oxidation roasted pellets after the oxidation roasted pellets are roasted at different oxidation roasting temperatures in the oxidation roasting section is detected. The compressive strength of the oxidation roasted pellets under different oxidation roasting temperatures T2 in the oxidation roasting section is obtained, and the relationship curve between the compressive strength and the roasting temperature T2 in the oxidation roasting section is plotted as shown in FIG. Figure 4 As shown, according to the curve fitting, the relationship between the compressive strength and the roasting temperature T2 in the oxidation roasting stage is: Y2=f(T2)= 0.00007*T2 3 - 0.2315*T2 2 + 249.12*T2- 91120.18.
[0034] The second step is to adjust the roasting time t2 of the oxidized pellets in the oxidized roasting section while ensuring that the roasting temperature in the roasting section remains unchanged, and detect the compressive strength of the oxidized pellets after roasting times t2 in different oxidized roasting sections. The compressive strength of the oxidized roasted pellets is obtained at different roasting times t2 in the oxidized roasting section, and a relationship curve between the compressive strength and the roasting time t2 of the oxidized roasted pellets in the oxidized roasting section is drawn as shown in FIG. Figure 5As shown, according to the curve fitting, the relationship between the compressive strength and the roasting time t2 of the oxidative roasting pellets in the oxidative roasting section is: Y2=f(t2)= 0.4640*t2 3 - 27.0708*t2 2 + 524.20*t2- 495.10.
[0035] The third step is to test the influence of each process condition on the compressive strength according to the two process conditions that affect the compressive strength of the oxidized pellets, set the influence factor of the process condition on the compressive strength and verify the accuracy, and obtain the temperature adjustment coefficient of the oxidized roasting process and the roasting time adjustment coefficient of the oxidized roasting process. The process conditions that affect the compressive strength of the oxidized roasted pellets in the entire oxidized roasting process are as follows: Y2=d*(0.00007*T2 3 - 0.2315*T2 2 + 249.12*T2- 91120.18) + e*(0.4640*t2 3 -27.0708*t2 2 + 524.20*t2- 495.10); Where: Y2 is the compressive strength of the oxidatively roasted pellets, N·P -1 ; T2 is the temperature in the roasting device, ℃; t2 is the roasting time of the oxidized pellets in the roasting device, h; d is the roasting process temperature adjustment coefficient; e is the roasting time adjustment coefficient; d+e=1.
[0036] According to the technical solution provided by the present invention, in actual production, the compressive strength requirement of the pre-oxidized pellets after the preheating process can be first set to Y 预设 (For example, the compressive strength of pre-oxidized pellets is not less than 500N·P -1 ), according to the specific preparation system and preparation conditions, calculate whether the compressive strength Y1 of the pre-oxidized pellets prepared under this process condition can reach Y 预设 If not, adjust the temperature in the preheating device, the residence time of the oxidized pellets in the preheating device, or the oxygen content in the gas in the preheating device so that the compressive strength Y1 of the preoxidized pellets prepared under this process condition is greater than or equal to Y 预设 .
[0037] According to the technical solution provided by the present invention, in actual production, the compressive strength requirement of the oxidatively roasted pellets after the roasting process can be first set to Y 氧设 (For example, the compressive strength of oxidatively roasted pellets is not less than 2300N·P -1), according to the specific preparation system and preparation conditions, calculate whether the compressive strength Y2 of the oxidative roasted pellets prepared under this process condition can reach Y 氧设 If not, adjust the temperature in the roasting device and the roasting time of the oxidized pellets in the roasting device so that the compressive strength Y2 of the oxidized roasted pellets prepared under this process condition is greater than or equal to Y 氧设 .
[0038] In the actual production process, the compressive strength requirement of the oxidative roasted pellets after the roasting process can also be directly set as Y3. According to the process conditions detected in the preheating process and the roasting process, the ideal compressive strength value Y of the material after the preheating process and the roasting process is calculated respectively. 预设 With Y 氧设 At the same time, the compressive strength Y3 (actual value) after the preheating and roasting parameters are coupled is obtained through the compressive strength test of representative pellet samples, and the three are compared: If Y3>Y2>Y1, it means that the process parameters of preheating and roasting for production meet the requirements, and no adjustment is required for the preheating process and the roasting process; If Y2>Y3>Y1, it indicates that the roasting parameters for production do not meet the expected requirements, and the process conditions of the roasting process need to be adjusted, such as increasing the roasting temperature, increasing the heat source in the roasting device, increasing the amount of fuel burned in the roasting device, increasing the number of microwave sources in the roasting device, and extending the roasting time. If Y2>Y1>Y3, it means that the coupling effect of the process conditions of the preheating process and the roasting process for production does not meet the expected requirements. It is preferred to adjust the roasting process to improve the roasting process parameters (such as increasing the roasting temperature, increasing the heat source in the roasting device, increasing the combustion amount of the fuel in the roasting device, increasing the number of microwave sources in the roasting device, and extending the roasting time), and then choose to adjust the process parameters of the preheating process (such as increasing the temperature of the circulating exhaust gas, increasing the oxygen enrichment concentration, and extending the residence time of the material in the preheating device).
[0039] In the present invention, the control of the preheating section and the control of the roasting section are obtained through experimental exploration and law summary by the inventor and can be generally applied.
[0040] In the technical means of controlling the preheating process, the formula fits the relationship between the compressive strength of the preoxidized pellets and the temperature in the preheating device, the residence time of the oxidized pellet materials in the preheating device, and the oxygen content in the gas in the preheating device. The three process conditions that can directly affect and have the greatest impact, namely, the temperature in the preheating device, the residence time of the oxidized pellet materials in the preheating device, and the oxygen content in the gas in the preheating device, are associated with the compressive strength of the oxidized pellets to obtain the relationship between the compressive strength of the preoxidized pellets and the process conditions in the preheating process. In the relationship, the parameters of the three process conditions, namely, the temperature in the preheating device, the residence time of the oxidized pellet materials in the preheating device, and the oxygen content in the gas in the preheating device, are converted into numerical values of agreed units and substituted into the relationship to obtain the compressive strength of the preoxidized pellets.
[0041] In the technical means of controlling the roasting process, the formula fits the relationship between the compressive strength of the oxidized roasted pellets and the temperature of the oxidized roasting process and the roasting time of the oxidized pellets in the roasting device. The temperature in the roasting device and the roasting time of the oxidized pellets in the roasting device, which are the two process conditions that can directly affect and have the greatest impact, are associated with the compressive strength of the oxidized roasted pellets to obtain the relationship between the compressive strength of the oxidized roasted pellets and the process conditions in the oxidized roasting process. In the relationship, the parameters of the two process conditions, the temperature in the roasting device and the roasting time of the oxidized pellets in the roasting device, are converted into numerical values of agreed units and substituted into the relationship to obtain the compressive strength of the oxidized roasted pellets.
[0042] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects: 1. The inventors of the present invention have explored the process conditions that have the greatest impact on the compressive strength of the pre-oxidized pellets in the preheating process of the oxidized pellets through research and experiments, and obtained the relationship between the compressive strength of the pre-oxidized pellets after the preheating process and the corresponding process conditions through formula fitting; 2. The inventors of the present invention have explored the process conditions that have the greatest impact on the compressive strength of the oxidized roasted pellets in the oxidized roasted pellet roasting process through research and experiments, and obtained the relationship between the compressive strength of the oxidized roasted pellets after the roasting process and the corresponding process conditions through formula fitting; 3. According to the compressive strength requirement of the oxidized pellets entering the blast furnace, the conditions of the oxidation preparation process are reasonably adjusted to ensure the compressive strength requirement of the oxidized pellets. The technical solution of the present invention has great significance for the actual production, avoids the dependence on the workers' experience, proposes a scientific control method, and avoids the intervention of human factors and the differences caused. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The graph is a relationship curve between the compressive strength of pre-oxidized pellets and the preheating temperature T1 in the preheating section in the oxidized pellet preparation process of the present invention.
[0044] Figure 2 It is a relationship curve between the compressive strength of pre-oxidized pellets and the residence time t1 of the oxidized pellet materials in the preheating section in the oxidized pellet preparation process of the present invention.
[0045] Figure 3 It is a relationship curve between the compressive strength of pre-oxidized pellets and the oxygen content C1 in the preheating device in the oxidation pellet preparation process of the present invention.
[0046] Figure 4 The graph is a relationship curve between the compressive strength of the oxidatively roasted pellets and the roasting temperature T2 in the oxidatively roasted section in the oxidatively roasted pellet preparation process of the present invention.
[0047] Figure 5 The graph is a relationship curve between the compressive strength of the oxidized roasted pellets and the roasting time t2 of the oxidized roasted pellets in the oxidized roasting section in the oxidized roasting process of the present invention.
[0048] In the attached drawings of the present invention, the curve of compressive strength detected under actual process conditions is implemented, and the dotted line is the relationship curve obtained by the inventor based on the actual process fitting. DETAILED DESCRIPTION
[0049] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments. Example 1
[0050] A process for preparing oxidized pellets, the process comprising the following steps: (1) Batching: The raw materials for oxidation pellets are mixed and pelletized to obtain oxidation pellet materials; (2) Preheating: The oxidized pellet material is transported to the preheating device, and the oxidized pellet material is preheated to obtain preoxidized pellets; wherein: the temperature in the preheating device, the residence time of the oxidized pellet material in the preheating device, and the oxygen content in the gas in the preheating device are controlled, so as to ensure the compressive strength of the preoxidized pellets after the oxidized pellet material passes through the preheating device; (3) Calcination: The pre-oxidized pellets are transported to a calcination device, and the pre-oxidized pellets are subjected to oxidative calcination to obtain oxidatively calcined pellets; wherein: the temperature in the calcination device and the calcination time of the pre-oxidized pellets in the calcination device are controlled, thereby ensuring the compressive strength of the oxidatively calcined pellets after the pre-oxidized pellets are calcined. Example 2
[0051] Example 1 was repeated, except that the control of step (2) was specifically as follows: Y1=a*(0.000005*T1 4 - 0.0195*T1 3 + 26.91*T1 2- 16453.06*T1+ 3757787.50) + b*(1.2308*t1 3 - 45.53*t1 2 + 575.16*t1- 1135.10) + c*(0.2671*C1 4 - 23.0660*C1 3 +736.06*C1 2 - 10211*C1+ 52534); Where: Y1 is the compressive strength of pre-oxidized pellets, N·P -1 ; T1 is the temperature in the preheating device, ℃; t1 is the residence time of the oxidized pellet material in the preheating device, h; C1 is the volume percentage of oxygen in the gas in the preheating device, %; a is the preheating process temperature adjustment coefficient; b is the preheating process residence time adjustment coefficient; c is the preheating process oxygen content adjustment coefficient; a+b+c=1. Example 3
[0052] Example 1 was repeated, except that the control of step (3) was specifically as follows: Y2=d*(0.00007*T2 3 - 0.2315*T2 2 + 249.12*T2- 91120.18) + e*(0.4640*t2 3 -27.0708*t2 2 + 524.20*t2- 495.10); Where: Y2 is the compressive strength of the oxidatively roasted pellets, N·P -1 ; T2 is the temperature in the roasting device, ℃; t2 is the roasting time of the oxidized pellets in the roasting device, h; d is the roasting process temperature adjustment coefficient; e is the roasting time adjustment coefficient; d+e=1. Example 4
[0053] Example 2 was repeated, except that the control of step (3) was specifically as follows: Y2=d*(0.00007*T2 3 - 0.2315*T2 2 + 249.12*T2- 91120.18) + e*(0.4640*t2 3 -27.0708*t2 2 + 524.20*t2- 495.10); Where: Y2 is the compressive strength of the oxidatively roasted pellets, N·P -1; T2 is the temperature in the roasting device, ℃; t2 is the roasting time of the oxidized pellets in the roasting device, h; d is the roasting process temperature adjustment coefficient; e is the roasting time adjustment coefficient; d+e=1.
[0054] Example 5
[0055] Example 4 was repeated, except that the value of a was 0.45, the value of b was 0.32, the value of c was 0.23, the value of d was 0.6, and the value of e was 0.4. Example 6
[0056] Example 4 is repeated, except that the preparation of the oxidized pellets adopts a chain grate and a rotary kiln system; the preheating device is a chain grate, and the preheating described in step (2) is completed in the chain grate; the roasting device is a rotary kiln, and the roasting described in step (3) is completed in the rotary kiln. Example 7
[0057] Example 4 is repeated, except that the preparation of the oxidized pellets is carried out using a belt roaster; the belt roaster includes a preheating section and a roasting section; the preheating device is the preheating section of the belt roaster, and the preheating described in step (2) is completed in the preheating section of the belt roaster; the roasting device is the roasting section of the belt roaster, and the roasting described in step (3) is completed in the roasting section of the belt roaster. Example 8
[0058] Example 4 is repeated, except that the preparation of the oxidized pellets is carried out in a vertical furnace; the vertical furnace includes a preheating section and a roasting section; the preheating device is the preheating section of the vertical furnace, and the preheating described in step (2) is completed in the preheating section of the vertical furnace; the roasting device is the roasting section of the vertical furnace, and the roasting described in step (3) is completed in the roasting section of the vertical furnace. Example 9
[0059] Example 8 was repeated, except that the vertical furnace was a vertical electric furnace; the vertical electric furnace was heated by microwaves.
[0060] Application Example Materials The technical solution of Example 5 is adopted to prepare oxidized pellets of the iron-containing material.
[0061] Among them: the raw materials of oxidized pellets: the iron-containing material is a mixture of a foreign magnetite concentrate and a domestic magnetite concentrate, accounting for 60% and 40% respectively, with a TFe content of about 63% and a -200 mesh content of about 90%.
[0062] The binder is bentonite, and its usage is 1%~2%.
[0063] The moisture content of raw balls is 8%~10%.
[0064] The raw materials are mixed in a powerful mixer for 45-60 seconds, and then pelletized in a disc pelletizer to obtain raw balls with a particle size of 10-15 mm and a compressive strength greater than 10 N·P -1 , the burst temperature is greater than 400℃.
[0065] According to the requirements of blast furnace feed and oxidation pellet preparation, the compressive strength requirement of the pre-oxidized pellet after preheating is set to 500N·P -1 above.
[0066] According to the blast furnace feed requirements, the compressive strength requirement for the oxidatively roasted pellets is set to 2500N·P -1 above.
[0067] The value of a is 0.45, the value of b is 0.32, the value of c is 0.23, the value of d is 0.6, and the value of e is 0.4.
[0068] Application Example 1 The technical solution of Example 6 was adopted, the temperature in the chain grate was detected to be 800° C., the residence time of the oxidized pellet material in the chain grate was 4 minutes, and the oxygen content in the chain grate was 18%.
[0069] After calculation, it is found that the compressive strength Y1 of the pre-oxidized pellets after preheating is 452 N·P -1 .
[0070] Under this process condition, the compressive strength requirement of the pre-oxidized pellets cannot be met. The temperature in the chain grate is adjusted to 900℃ and the residence time is 5min, so that the compressive strength Y1 of the pre-oxidized pellets after preheating reaches 840 N·P -1 .
[0071] Application Example 2 The technical solution of Example 8 was adopted, and the temperature of the preheating section in the electric furnace was detected to be 900° C., the residence time of the oxidized pellet material in the preheating section of the electric furnace was 6 minutes, and the oxygen content in the preheating section of the electric furnace was 20%.
[0072] After calculation, it is found that the compressive strength Y1 of the pre-oxidized pellets after preheating is 951 N·P -1 .
[0073] Under this process condition, the compressive strength requirement of the pre-oxidized pellets after preheating is met, and the preheating process is continued according to this process.
[0074] Application Example 3 The technical solution of Example 6 was adopted, the temperature in the chain grate was detected to be 950° C., the residence time of the oxidized pellet material in the chain grate was 8 min, and the oxygen content in the chain grate was 20%.
[0075] After calculation, it is found that the compressive strength Y1 of the pre-oxidized pellets after preheating is 1167 N·P -1 .
[0076] Under this process condition, the compressive strength requirement of the pre-oxidized pellets after preheating is met, and the preheating process is continued according to this process.
[0077] The temperature in the rotary kiln was detected to be 1250°C, and the residence time of the oxidized pellets in the rotary kiln was 20 minutes.
[0078] After calculation, the compressive strength Y2 of the oxidized pellets after preheating is 2152 N·P -1 .
[0079] Under this process condition, the compressive strength requirement of the oxidized roasted pellets after roasting cannot be met. The temperature in the rotary kiln is adjusted to 1300℃, so that the compressive strength Y2 of the oxidized roasted pellets after roasting reaches 2636 N·P -1 .
[0080] Application Example 4 Using the technical solution of Application Example 2, the temperature of the roasting section in the electric furnace was detected to be 1330° C., and the residence time of the oxidized pellets in the roasting section of the electric furnace was 25 minutes.
[0081] After calculation, the compressive strength Y2 of the oxidized roasted pellets after roasting is 3030 N·P -1 .
[0082] Under the process conditions, the compressive strength requirements of the oxidative roasting pellets after roasting are met, and the oxidative roasting process is continued according to this process.
Claims
1. A process for preparing oxidation pellets, the preparation process The following steps are involved: (1) Batching: The raw materials for oxidation pellets are mixed and pelletized to obtain oxidation pellet materials; (2) Preheating: The oxidized pellet material is transported to the preheating device, and the oxidized pellet material is preheated to obtain preoxidized pellets; wherein: the temperature in the preheating device, the residence time of the oxidized pellet material in the preheating device, and the oxygen content in the gas in the preheating device are controlled, so as to ensure the compressive strength of the preoxidized pellets after the oxidized pellet material passes through the preheating device; (3) Calcination: The pre-oxidized pellets are transported to a calcination device, and the pre-oxidized pellets are subjected to oxidative calcination to obtain oxidatively calcined pellets; wherein: the temperature in the calcination device and the calcination time of the pre-oxidized pellets in the calcination device are controlled, thereby ensuring the compressive strength of the oxidatively calcined pellets after the pre-oxidized pellets are calcined.
2. The process for preparing oxidized pellets according to claim 1, Features: The relationship between the compressive strength of the pre-oxidized pellets and the temperature in the preheating device, the residence time of the oxidized pellets in the preheating device, and the oxygen content in the gas in the preheating device is: Y 1 =a*(0.000005*T 1 4 - 0.0195*T 1 3 + 26.91*T 1 2 - 16453.06*T 1 + 3757787.50) + b*(1.2308*t 1 3 - 45.53*t 1 2 + 575.16*t 1 - 1135.10) + c*(0.2671*C 1 4 - 23.0660*C 1 3 +736.06*C 1 2 - 10211*C 1 + 52534); Where: Y 1 is the compressive strength of pre-oxidized pellets, N·P -1 ; T 1 is the temperature in the preheating device, °C; t 1 is the residence time of the oxidized pellets in the preheating device, h; C 1 is the volume percentage of oxygen in the gas in the preheating device, %; a is the preheating process temperature adjustment coefficient; b is the preheating process residence time adjustment coefficient; c is the preheating process oxygen content adjustment coefficient; a+b+c=1.
3. The process for preparing oxidized pellets according to claim 1, Features: The relationship between the compressive strength of the oxidized roasted pellets and the temperature in the roasting device and the roasting time of the pre-oxidized pellets in the roasting device is: Y 2 =d*(0.00007*T 2 3 - 0.2315*T 2 2 + 249.12*T 2 - 91120.18) + e*(0.4640*t 2 3 -27.0708*t 2 2 + 524.20*t 2 - 495.10); Where: Y 2 is the compressive strength of oxidatively roasted pellets, N·P -1 ; T 2 is the temperature in the roasting device, °C; t 2 is the roasting time of the oxidized pellets in the roasting device, h; d is the roasting process temperature adjustment coefficient; e is the roasting time adjustment coefficient; d+e=1.
4. The process for preparing oxidized pellets according to claim 2, Features: a>b>c; Preferably, the value of a is 0.4-0.5, the value of b is 0.3-0.35, and the value of c is 0.15-0.
3.
5. The process for preparing oxidized pellets according to claim 3, Features: d>e; Preferably, the value of d is 0.55-0.65, and the value of e is 0.35-0.
45.
6. The process for preparing oxidized pellets according to any one of claims 1 to 5, Features: The preparation of the oxidized pellets adopts a chain grate-rotary kiln system; the preheating device is a chain grate, and the preheating in step (2) is completed in the chain grate; the roasting device is a rotary kiln, and the roasting in step (3) is completed in the rotary kiln; or The preparation of the oxidized pellets is completed by a belt roasting machine; the belt roasting machine includes a preheating section and a roasting section; the preheating device is the preheating section of the belt roasting machine, and the preheating described in step (2) is completed in the preheating section of the belt roasting machine; the roasting device is the roasting section of the belt roasting machine, and the roasting described in step (3) is completed in the roasting section of the belt roasting machine.
7. The process for preparing oxidized pellets according to any one of claims 1 to 6, Features: The preparation of the oxidized pellets is completed in a vertical furnace; the vertical furnace includes a preheating section and a roasting section; the preheating device is the preheating section of the vertical furnace, and the preheating in step (2) is completed in the preheating section of the vertical furnace; the roasting device is the roasting section of the vertical furnace, and the roasting in step (3) is completed in the roasting section of the vertical furnace.
8. The process for preparing oxidized pellets according to claim 7, Features: The vertical furnace is a vertical electric furnace; preferably, the vertical electric furnace is heated by microwaves.
9. The process for preparing oxidized pellets according to any one of claims 1 to 5, Features: The compressive strength of pre-oxidized pellets is not less than 500N·P -1 ; and / or The compressive strength of oxidatively roasted pellets is not less than 2300N·P -1 .
10. The process for preparing oxidized pellets according to any one of claims 1 to 9, Features: The raw material for oxidized pellets is an iron-containing material; optionally, it also includes one or more of a fuel, a binder, and water.