Recycling method of molybdenum alloy offcuts

Through annealing, sandblasting, crushing, hydrogenation and dehydrogenation treatment, the molybdenum alloy edge material is converted into molybdenum alloy powder with low hydrogen content and low oxygen content, which solves the problem of the failure of effective recycling of molybdenum alloy edge material and improves the finished material and reduce production costs.

CN118910412APending Publication Date: 2024-11-08KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411005535.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The failure of the prior art to effectively utilize molybdenum alloy edges has resulted in the failure to effectively recycle and use the scraps and residual targets it produces in production, wasting resources and increasing production costs.

Method used

Through annealing, sandblasting, crushing, hydrogenation, screening and dehydrogenation, the molybdenum alloy edge material is converted into molybdenum alloy powder with low hydrogen content and low oxygen content. It is suitable for the reproduction of molybdenum alloy targets and improves the yield And reduce production costs.

Benefits of technology

It has achieved efficient recycling of molybdenum alloy edge materials, low hydrogen content and oxygen content, and a material yield of up to 85%, greatly saving the production cost of molybdenum alloy targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910412A_ABST
    Figure CN118910412A_ABST
Patent Text Reader

Abstract

The invention provides a molybdenum alloy offcut recovery method which comprises the following steps: (1) sequentially carrying out annealing treatment, sand blasting treatment and first crushing treatment on molybdenum alloy offcuts, and then carrying out hydrotreating to obtain a hydrogenated material; and (2) the hydrogenated material is sequentially subjected to second crushing treatment, screening treatment and dehydrogenation treatment, and the dehydrogenated molybdenum alloy powder is obtained. According to the recovery method, the molybdenum alloy offcut is made into the molybdenum alloy powder, the molybdenum alloy powder can be reused in production of the molybdenum alloy target material, the yield is high, and the production cost of the molybdenum alloy target material is greatly saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sputtering target materials, and in particular to a method for recovering molybdenum alloy edge material. Background Art

[0002] Molybdenum alloy targets are generally used in the LCD flat panel display industry. Currently, as display panels develop towards high-generation lines and OLEDs, the trend of conductive materials shifting from aluminum to copper is taking shape. Molybdenum / molybdenum alloys and copper have excellent adhesion, which is beneficial to the stability of the barrier layer. Therefore, the use of molybdenum alloys is increasing. However, a certain amount of scraps will be generated during the production of molybdenum alloys, and there will be a large amount of residual targets after use, which can basically reach 20-30% of the raw material input. There is currently no effective method for recycling them.

[0003] CN114087875A discloses a molybdenum alloy smelting and recovery equipment and a vacuum degassing and impurity removal smelting furnace, including a main support frame and a vacuum degassing and impurity removal smelting furnace mounting frame, a vacuum refining furnace is arranged on the main support frame, a vacuum degassing and impurity removal smelting furnace is installed in the vacuum degassing and impurity removal smelting furnace mounting frame, the vacuum refining furnace is located directly below the vacuum degassing and impurity removal smelting furnace, and a crystallization device and an ingot pulling device are arranged in sequence below the vacuum refining furnace. A molybdenum alloy smelting and recovery method is also provided, which includes four steps of preparing consumable electrodes, vacuum degassing and impurity removal, refining and preparing recovered molybdenum alloy blocks. The molybdenum alloy smelting and recovery equipment can improve the purity of the recovered molybdenum alloy blocks and improve the smelting efficiency at the same time.

[0004] CN102277494A discloses a dissolving, separating and recovering process of uranium-molybdenum alloy in uranium-molybdenum / aluminum dispersed fuel elements. The process comprises cleaning and cutting the fuel elements, heating them at 60 to 100°C with a concentration of 20.0 to 80.0 g L -1 The concentration of NaOH is 60.0~100.0g L -1 The uranium-molybdenum alloy powder is obtained by dissolving the aluminum alloy in a mixed solution of NaNO3, cooling the dissolved solution, letting it stand, filtering and washing it, and separating the dissolved solution from the insoluble solid. The process can dissolve all the aluminum alloy into the solution phase, effectively reducing the loss rate of uranium, and the uranium recovery rate reaches more than 99.3%. The separated uranium-molybdenum alloy powder can be returned for reuse after treatment, reducing production costs.

[0005] CN1037932A discloses a new method for recovering molybdenum sheets, which uses a No. 1 etching solution prepared with deionized water, hydrofluoric acid and hydrogen peroxide and a No. 2 etching solution prepared with sodium hydroxide and hydrogen peroxide to corrode and remove the aluminum-silicon-molybdenum alloy on the molybdenum sheets.

[0006] The above-mentioned recycling methods for molybdenum alloys cannot fully utilize their maximum utilization value. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a method for recycling molybdenum alloy scraps, which can be reused in the production of molybdenum alloy targets by making them into molybdenum alloy powder, thus maximizing their utilization value and greatly saving the preparation cost of molybdenum alloy targets.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for recycling molybdenum alloy scraps, the method comprising the following steps:

[0010] (1) the molybdenum alloy edge material is subjected to annealing treatment, sandblasting treatment and first crushing treatment in sequence, and then subjected to hydrogenation treatment to obtain a hydrogenated material;

[0011] (2) The hydrogenated material is subjected to a second crushing treatment, a screening treatment and a dehydrogenation treatment in sequence to obtain a dehydrogenated molybdenum alloy powder; the dehydrogenated molybdenum alloy powder has a hydrogen content of less than 220 ppm and an oxygen content of less than 1500 ppm.

[0012] The molybdenum alloy scrap recycling method of the present invention can be applied to scraps and residual targets of molybdenum-niobium target materials, molybdenum-titanium target materials, molybdenum-titanium-nickel target materials, and molybdenum-tantalum target materials. The recycling method first anneals the molybdenum alloy scraps to improve their brittleness and facilitate subsequent crushing; sandblasts the annealed molybdenum alloy scraps to remove stains and oxide layers attached to the surface to ensure that the scraps are completely exposed to metallic color; then performs a first crushing treatment, a hydrogenation treatment, a second crushing treatment, a screening treatment, and a dehydrogenation treatment to make the molybdenum alloy scraps into molybdenum alloy powder. The dehydrogenated molybdenum alloy powder has low hydrogen content and low oxygen content, can be reused in the production of molybdenum alloy targets, and has a high yield rate, which greatly saves the production cost of molybdenum alloy targets.

[0013] The hydrogen content of the dehydrogenated molybdenum alloy powder of the present invention is less than 220 ppm, for example, it can be 219 ppm, 210 ppm, 200 ppm, 190 ppm, 150 ppm, 100 ppm or 50 ppm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0014] The oxygen content is less than 1500 ppm, for example, it can be 1499 ppm, 1400 ppm, 1300 ppm, 1100 ppm, 1000 ppm, 900 ppm or 500 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] Preferably, the vacuum degree of the annealing treatment in step (1) is below 10 Pa, for example, it can be 9.9 Pa, 9.5 Pa, 9 Pa, 8 Pa, 7 Pa, 5 Pa or 3 Pa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the annealing temperature is 1000-1200°C, for example, 1000°C, 1050°C, 1100°C, 1130°C, 1150°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0017] The present invention preferably uses an annealing temperature of 1000-1200°C, in which the molybdenum alloy material can be fully alloyed and its brittleness can be increased. When the annealing temperature is low, it still has great toughness, which will lead to subsequent crushing difficulties; when the annealing temperature is high, the brittleness of the material is not significantly increased compared with the 1000-1200°C process, and the equipment requirements are higher, wasting energy.

[0018] Preferably, the annealing treatment time is 2 to 6 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 5 hours or 6 hours, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, after the sandblasting in step (1), the molybdenum alloy edge material is ultrasonically cleaned with anhydrous ethanol for 10 to 15 minutes, for example, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 14.5 minutes or 15 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] Preferably, the particle size of the molybdenum alloy edge material after the first crushing treatment in step (1) is below 50 mm, for example, it can be 49 mm, 45 mm, 40 mm, 30 mm, 20 mm or 10 mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the heating rate of the hydrogenation treatment in step (1) is 5 to 8°C / min, for example, 5°C / min, 5.5°C / min, 6°C / min, 7°C / min, 7.5°C / min or 8°C / min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] The present invention preferably uses a heating rate of 5 to 8°C / min for hydrogenation treatment, which can fully activate the molybdenum alloy material, increase the hydrogen absorption, and facilitate subsequent crushing. When the heating rate of hydrogenation treatment is slow, the hydrogenation process will take too long and the efficiency will be too low; when the heating rate of hydrogenation treatment is fast, the molybdenum alloy material will not be hydrogenated enough and will be difficult to crush.

[0023] When the temperature rises to 500-700°C, hydrogen is introduced. For example, it can be 500°C, 550°C, 600°C, 620°C, 650°C, 680°C or 700°C, but it is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the pressure of the hydrogenation treatment is 0.05-0.08 MPa, for example, it can be 0.05 MPa, 0.055 MPa, 0.06 MPa, 0.065 MPa, 0.07 MPa, 0.075 MPa or 0.08 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the hydrogenation treatment time is 5 to 10 h, for example, 5 h, 5.5 h, 6 h, 6.5 h, 8 h or 10 h, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, after the hydrogenation treatment is completed, the temperature is lowered to below 300°C and the introduction of hydrogen is stopped. The hydrogenated material is obtained after cooling. For example, the temperature may be 299°C, 290°C, 280°C, 250°C, 200°C, 150°C or 100°C, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the particle size of the hydrogenated material after the second crushing treatment in step (2) is less than 10 mm, for example, it can be 9.9 mm, 8 mm, 5 mm, 3 mm, 2 mm or 1 mm, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the screening process in step (2) is performed using a sieve of 200 to 300 mesh, for example, 200 mesh, 230 mesh, 250 mesh, 280 mesh or 300 mesh, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the screened material after the screening treatment is returned to the hydrogenation treatment in step (1).

[0030] Preferably, the vacuum degree of the dehydrogenation treatment in step (2) is less than 5 Pa, for example, it can be 4.9 Pa, 4.5 Pa, 4 Pa, 3 Pa, 2 Pa, 1 Pa or 0.1 Pa, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the hydrogenated material subjected to the dehydrogenation treatment is placed in layers, and the thickness of each powder layer does not exceed 15 mm, for example, it can be 14.9 mm, 14.5 mm, 14 mm, 13 mm, 12 mm or 10 mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the temperature of the dehydrogenation treatment is 700-900°C, for example, it can be 700°C, 750°C, 800°C, 820°C, 850°C, 880°C or 900°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] The preferred dehydrogenation temperature of the present invention is 700-900°C, which allows the hydrogenated material to be fully dehydrogenated and the hydrogen content of the final product to be as low as possible. When the dehydrogenation temperature is low, the dehydrogenation effect is poor and the dehydrogenation is incomplete; when the dehydrogenation temperature is high, the powders will be sintered together.

[0034] Preferably, the dehydrogenation treatment time is 8 to 15 hours, for example, 8 hours, 8.5 hours, 9 hours, 10 hours, 12 hours or 15 hours, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the particle size of the dehydrogenated molybdenum alloy powder in step (2) is below 100 μm, for example, it can be 99 μm, 90 μm, 80 μm, 70 μm, 60 μm or 50 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] As a preferred technical solution of the present invention, the recovery method comprises the following steps:

[0037] (1) The molybdenum alloy edge material is subjected to annealing treatment at a vacuum degree of less than 10 Pa and a temperature of 1000-1200° C. for 2-6 h, sandblasting treatment and a first crushing treatment, and then subjected to hydrogenation treatment at a pressure of 0.05-0.08 MPa for 5-10 h. After the hydrogenation treatment is completed, the temperature is lowered to below 300° C. and the introduction of hydrogen is stopped. After cooling, a hydrogenated material is obtained;

[0038] The molybdenum alloy edge material after the sandblasting treatment is ultrasonically cleaned with anhydrous ethanol for 10 to 15 minutes; the particle size of the molybdenum alloy edge material after the first crushing treatment is less than 50 mm;

[0039] The heating rate of the hydrogenation treatment is 5-8°C / min, and hydrogen is introduced when the temperature rises to 500-700°C;

[0040] (2) The hydrogenated material is sequentially subjected to a second crushing treatment, a screening treatment, and a dehydrogenation treatment at a vacuum degree of <5 Pa and a temperature of 700 to 900° C. for 8 to 15 hours to obtain a dehydrogenated molybdenum alloy powder with a particle size of less than 100 μm; the dehydrogenated molybdenum alloy powder has a hydrogen content of less than 220 ppm and an oxygen content of less than 1500 ppm;

[0041] The screening process is performed using a sieve of 200 to 300 meshes; the screened material after the screening process is returned to the hydrogenation process in step (1); the hydrogenated material from the dehydrogenation process is placed in layers, and the thickness of each layer of powder does not exceed 15 mm.

[0042] Compared with the prior art, the present invention has at least the following beneficial effects:

[0043] The molybdenum alloy scrap recovery method provided by the present invention makes the molybdenum alloy scrap into molybdenum alloy powder. The molybdenum alloy powder has low hydrogen and oxygen contents and can be reused in the production of molybdenum alloy target materials. The yield rate is as high as over 85%, which greatly saves product production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 The present invention is a schematic flow diagram of a method for recycling molybdenum alloy scraps. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0046] The present invention provides a method for recycling molybdenum alloy scraps, the schematic diagram of which is as follows: Figure 1 shown.

[0047] The recovery method comprises the following steps:

[0048] (1) the molybdenum alloy edge material is subjected to annealing treatment, sandblasting treatment and first crushing treatment in sequence, and then subjected to hydrogenation treatment to obtain a hydrogenated material;

[0049] (2) The hydrogenated material is sequentially subjected to a second crushing process, a screening process and a dehydrogenation process to obtain a dehydrogenated molybdenum alloy powder.

[0050] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0051] Example 1

[0052] The present embodiment provides a method for recycling molybdenum alloy scraps, the method comprising the following steps:

[0053] (1) The molybdenum alloy edge material is subjected to annealing treatment at a vacuum degree of 8 Pa and a temperature of 1100° C. for 3 h, sandblasting treatment, and a first crushing treatment, and then subjected to a hydrogenation treatment at a pressure of 0.07 MPa for 8 h. After the hydrogenation treatment, the temperature is lowered to 250° C. and the introduction of hydrogen is stopped. After cooling, a hydrogenated material is obtained;

[0054] The molybdenum alloy edge material after the sandblasting treatment is ultrasonically cleaned for 13 minutes using anhydrous ethanol; the particle size of the molybdenum alloy edge material after the first crushing treatment is 30 mm;

[0055] The heating rate of the hydrogenation treatment is 6°C / min, and hydrogen is introduced when the temperature reaches 600°C;

[0056] (2) The hydrogenated material is subjected to a second crushing process, a screening process, and a dehydrogenation process at a vacuum degree of less than 3 Pa and a temperature of 750° C. for 10 h to obtain a dehydrogenated molybdenum alloy powder with a particle size of 50 μm;

[0057] The screening process is performed using a 250-mesh screen; the screened material after the screening process is returned to the hydrogenation process in step (1); the hydrogenated material from the dehydrogenation process is placed in layers, and the thickness of each layer of powder is 10 mm.

[0058] Example 2

[0059] The present embodiment provides a method for recycling molybdenum alloy scraps, the method comprising the following steps:

[0060] (1) The molybdenum alloy edge material is subjected to annealing treatment at a vacuum degree of 4 Pa ​​and a temperature of 1000° C. for 6 h, sandblasting treatment, and a first crushing treatment, and then subjected to a hydrogenation treatment at a pressure of 0.08 MPa for 10 h. After the hydrogenation treatment, the temperature is lowered to 220° C. and the introduction of hydrogen is stopped. After cooling, a hydrogenated material is obtained;

[0061] The molybdenum alloy edge material after the sandblasting treatment is ultrasonically cleaned with anhydrous ethanol for 10 minutes; the particle size of the molybdenum alloy edge material after the first crushing treatment is 40 mm;

[0062] The heating rate of the hydrogenation treatment is 5°C / min, and hydrogen is introduced when the temperature rises to 500°C;

[0063] (2) The hydrogenated material is subjected to a second crushing treatment, a screening treatment, and a dehydrogenation treatment at a vacuum degree of 2 Pa and a temperature of 700° C. for 15 h to obtain a dehydrogenated molybdenum alloy powder with a particle size of 80 μm;

[0064] The screening process is performed using a 300-mesh screen; the screened material after the screening process is returned to the hydrogenation process in step (1); the hydrogenated material from the dehydrogenation process is placed in layers, and the thickness of each layer of powder is 11 mm.

[0065] Example 3

[0066] The present embodiment provides a method for recycling molybdenum alloy scraps, the method comprising the following steps:

[0067] (1) The molybdenum alloy edge material is subjected to annealing treatment at a vacuum degree of 3 Pa and a temperature of 1200° C. for 2 h, sandblasting treatment, and a first crushing treatment, and then subjected to a hydrogenation treatment at a pressure of 0.05 MPa for 5 h. After the hydrogenation treatment, the temperature is lowered to 260° C. and the introduction of hydrogen is stopped. After cooling, a hydrogenated material is obtained;

[0068] The molybdenum alloy edge material after the sandblasting treatment is ultrasonically cleaned for 15 minutes using anhydrous ethanol; the particle size of the molybdenum alloy edge material after the first crushing treatment is 20 mm;

[0069] The heating rate of the hydrogenation treatment is 8°C / min, and hydrogen is introduced when the temperature reaches 700°C;

[0070] (2) The hydrogenated material is subjected to a second crushing treatment, a screening treatment, and a dehydrogenation treatment at a vacuum degree of 4 Pa ​​and a temperature of 900° C. for 8 h to obtain a dehydrogenated molybdenum alloy powder with a particle size of 60 μm;

[0071] The screening process is performed using a 200-mesh screen; the screened material after the screening process is returned to the hydrogenation process in step (1); the hydrogenated material from the dehydrogenation process is placed in layers, and the thickness of each layer of powder is 10 mm.

[0072] Example 4

[0073] This embodiment provides a method for recovering molybdenum alloy scraps. The method is the same as that of Embodiment 1 except that the heating rate of the hydrogenation treatment in step (1) is 4°C / min.

[0074] Example 5

[0075] This embodiment provides a method for recovering molybdenum alloy scraps. The method is the same as that of Embodiment 1 except that the heating rate of the hydrogenation treatment in step (1) is 9°C / min.

[0076] Example 6

[0077] This embodiment provides a method for recovering molybdenum alloy scraps. The method is the same as that of Embodiment 1 except that the temperature of the dehydrogenation treatment in step (2) is 600°C.

[0078] Example 7

[0079] This embodiment provides a method for recovering molybdenum alloy scraps. The method is the same as that of Embodiment 1 except that the temperature of the dehydrogenation treatment in step (2) is 1000°C.

[0080] Comparative Example 1

[0081] This comparative example provides a method for recycling molybdenum alloy scraps. The recycling method is the same as Example 1 except that step (1) does not involve annealing.

[0082] Comparative Example 2

[0083] This comparative example provides a method for recycling molybdenum alloy scraps. The recycling method is the same as Example 1 except that the annealing temperature in step (1) is 900°C.

[0084] Comparative Example 3

[0085] This comparative example provides a method for recycling molybdenum alloy scraps. The recycling method is the same as Example 1 except that the annealing temperature in step (1) is 1300°C.

[0086] The hydrogen content, oxygen content and yield rate of the dehydrogenated molybdenum alloy powder obtained in the above examples and comparative examples were measured, and the results are shown in Table 1.

[0087] Table 1

[0088] Hydrogen content (ppm) Oxygen content (ppm) Yield rate (%) Example 1 126 1032 94 Example 2 138 1125 93 Example 3 145 1089 92 Example 4 163 1360 88 Example 5 175 1295 87 Example 6 215 1386 88 Example 7 201 1433 83 Comparative Example 1 152 1260 58 Comparative Example 2 143 1312 73 Comparative Example 3 148 1678 92

[0089] From Table 1 we can see that:

[0090] (1) It can be seen from Examples 1 to 3 that the method for recovering molybdenum alloy scrap provided by the present invention obtains high-quality dehydrogenated molybdenum alloy powder with low hydrogen content and low oxygen content, which can be reused in the production of molybdenum alloy target materials with high yield rate, thus greatly saving the production cost of molybdenum alloy target materials;

[0091] (2) It can be seen from the combination of Example 1 and Examples 4 to 5 that the heating rate of the hydrogenation treatment in Example 4 is relatively slow, which will lead to a long hydrogenation process time and low efficiency, and the hydrogen content of the obtained dehydrogenated molybdenum alloy powder is relatively high, which is 163ppm, and the oxygen content is also relatively high, which is 1360ppm, and the yield rate is reduced to 88%; the heating rate of the hydrogenation treatment in Example 5 is relatively fast, the degree of hydrogenation of the molybdenum alloy material is insufficient, and it is difficult to crush. The hydrogen content of the obtained dehydrogenated molybdenum alloy powder is relatively high, which is 175ppm, and the oxygen content is also relatively high, which is 1295ppm, and the yield rate is reduced to 87%;

[0092] (3) Combining Example 1 with Examples 6 to 7, it can be seen that the temperature of the dehydrogenation treatment in Example 6 is relatively low, which will lead to poor dehydrogenation effect and incomplete dehydrogenation. The hydrogen content of the dehydrogenated molybdenum alloy powder obtained is relatively high, which is 215ppm, and the oxygen content is also relatively high, which is 1386ppm. The yield rate is reduced to 88%. The temperature of the dehydrogenation treatment in Example 7 is relatively high, which will cause the powder to be sintered together.

[0093] (4) It can be seen from the combination of Example 1 and Comparative Examples 1 to 3 that Comparative Example 1 does not undergo annealing treatment, and the annealing temperature in Comparative Example 2 is relatively low, both of which lead to subsequent difficulty in crushing. The yield rates of Comparative Examples 1 and 2 are greatly reduced, which are 58% and 73%, respectively. The annealing temperature in Comparative Example 3 is relatively high, and the brittleness of the material is not significantly increased compared to the 1000-1200°C process, but the equipment requirements are higher, wasting energy.

[0094] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for recovering molybdenum alloy edge material, characterized in that: The recovery method comprises the following steps: (1) the molybdenum alloy edge material is subjected to annealing treatment, sandblasting treatment and first crushing treatment in sequence, and then subjected to hydrogenation treatment to obtain a hydrogenated material; (2) the hydrogenated material is subjected to a second crushing treatment, a screening treatment and a dehydrogenation treatment in sequence to obtain a dehydrogenated molybdenum alloy powder; the screened material after the screening treatment is returned to the hydrogenation treatment in step (1); The dehydrogenated molybdenum alloy powder has a hydrogen content of less than 220 ppm and an oxygen content of less than 1500 ppm.

2. The recycling method according to claim 1, characterized in that: The vacuum degree of the annealing treatment in step (1) is below 10 Pa; Preferably, the temperature of the annealing treatment is 1000-1200°C; Preferably, the annealing treatment time is 2 to 6 hours.

3. The recovery method according to claim 1 or 2, characterized in that: After the sandblasting treatment in step (1), the molybdenum alloy edge material is ultrasonically cleaned for 10 to 15 minutes using anhydrous ethanol.

4. The recycling method according to any one of claims 1 to 3, characterized in that: Step (1) After the first crushing treatment, the particle size of the molybdenum alloy edge material is less than 50 mm.

5. The recycling method according to any one of claims 1 to 4, characterized in that: The heating rate of the hydrogenation treatment in step (1) is 5-8°C / min, and hydrogen is introduced when the temperature rises to 500-700°C; Preferably, the pressure of the hydrogenation treatment is 0.05-0.08 MPa; Preferably, the hydrogenation treatment time is 5 to 10 hours; Preferably, after the hydrogenation treatment is completed, the temperature is lowered to below 300° C., the introduction of hydrogen is stopped, and the hydrogenated material is obtained after cooling.

6. The recycling method according to any one of claims 1 to 5, characterized in that: Step (2) The particle size of the hydrogenated material after the second crushing treatment is less than 10 mm.

7. The recycling method according to any one of claims 1 to 6, characterized in that: The screening process in step (2) is carried out using a sieve of 200 to 300 meshes.

8. The recovery method according to any one of claims 1 to 7, characterized in that: The vacuum degree of the dehydrogenation treatment in step (2) is less than 5 Pa; Preferably, the dehydrogenated medium material is placed in layers, and the thickness of each layer of powder does not exceed 15 mm; Preferably, the temperature of the dehydrogenation treatment is 700-900°C; Preferably, the dehydrogenation treatment time is 8 to 15 hours.

9. The recycling method according to any one of claims 1 to 8, characterized in that: The particle size of the dehydrogenated molybdenum alloy powder in step (2) is below 100 μm.

10. The recycling method according to any one of claims 1 to 9, characterized in that: The recovery method comprises the following steps: (1) The molybdenum alloy edge material is subjected to annealing treatment at a vacuum degree of less than 10 Pa and a temperature of 1000-1200° C. for 2-6 h, sandblasting treatment and a first crushing treatment, and then subjected to hydrogenation treatment at a pressure of 0.05-0.08 MPa for 5-10 h. After the hydrogenation treatment is completed, the temperature is lowered to below 300° C. and the introduction of hydrogen is stopped. After cooling, a hydrogenated material is obtained; The molybdenum alloy edge material after the sandblasting treatment is ultrasonically cleaned with anhydrous ethanol for 10 to 15 minutes; the particle size of the molybdenum alloy edge material after the first crushing treatment is less than 50 mm; The heating rate of the hydrogenation treatment is 5-8°C / min, and hydrogen is introduced when the temperature rises to 500-700°C; (2) The hydrogenated material is sequentially subjected to a second crushing treatment, a screening treatment, and a dehydrogenation treatment at a vacuum degree of <5 Pa and a temperature of 700 to 900° C. for 8 to 15 hours to obtain a dehydrogenated molybdenum alloy powder with a particle size of less than 100 μm; the dehydrogenated molybdenum alloy powder has a hydrogen content of less than 220 ppm and an oxygen content of less than 1500 ppm; The screening process is performed using a sieve of 200 to 300 meshes; the screened material after the screening process is returned to the hydrogenation process in step (1); the hydrogenated material from the dehydrogenation process is placed in layers, and the thickness of each layer of powder does not exceed 15 mm.