Industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode material

Through the acid leaching treatment of oxalic acid aqueous solution and magnesium chloride and ammonia water, combined with the vanadium precipitation reaction of ammonium chloride, the efficient recycling of vanadium and phosphorus in waste vanadium sodium phosphate positive electrode materials was successfully achieved, and the low recycling efficiency and environment in the existing technology were solved. The problem of pollution has obtained high-purity vanadium pentoxide, which is suitable for industrial-grade applications.

CN118910430APending Publication Date: 2024-11-08HUBEI UNIV OF TECH

Patent Information

Application Number
CN202410932472.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, when recycling waste sodium vanadium phosphate positive electrode materials, the recycling efficiency of vanadium and phosphorus is low, the use of extractant is high and harmful to the environment, and the strong acid corrosion equipment in the acid leach process limits industrial-grade large-scale applications.

Method used

The acid leaching treatment was performed using aqueous oxalic acid solution, magnesium chloride and ammonia water were added for phosphorus precipitation reaction, followed by ammonium chloride for vanadium precipitation reaction, and vanadium dipentoxide was obtained by calcining, and phosphorus was removed by generating ammonium magnesium phosphate, optimizing the recovery of vanadium process.

Benefits of technology

It realizes efficient recycling of vanadium and phosphorus, reduces costs, improves the purity and electrochemical properties of vanadium pentoxide, reduces environmental pollution, and is suitable for industrial-grade large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910430A_ABST
    Figure CN118910430A_ABST
Patent Text Reader

Abstract

The invention discloses an industrial-grade method for recovering vanadium and phosphorus from a waste sodium vanadium phosphate positive electrode material, and belongs to the technical field of regeneration of useful parts of waste storage batteries. The method comprises the following steps: (1) carrying out discharge treatment on the waste sodium-ion battery to enable the waste sodium-ion battery to discharge completely, and disassembling and recycling to obtain a sodium vanadium phosphate material; (2) the sodium vanadium phosphate material is added into an oxalic acid aqueous solution for acid leaching treatment, and a sodium vanadium phosphate acid leaching solution is obtained; (3) adding a magnesium chloride aqueous solution into the sodium vanadium phosphate acid leaching solution, adjusting the pH value of the system by using ammonia water, carrying out phosphorus precipitation reaction, and recovering generated magnesium ammonium phosphate precipitate to obtain a dephosphorized solution; (4) adding an ammonium chloride aqueous solution into the dephosphorization solution to adjust the pH value of the system, carrying out vanadium precipitation reaction, and recovering to obtain ammonium metavanadate precipitate; and (5) calcining and oxidizing the ammonium metavanadate precipitate in an aerobic environment to obtain vanadium pentoxide. The recycling process of the method has the advantages of safety, high efficiency, high recycling rate and suitability for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of regeneration of useful parts of waste batteries, and in particular to an industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode materials. Background Art

[0002] In the past two decades, the technology and industry of lithium-ion batteries have made great progress around the world. Compared with the previous lead-acid batteries, lithium-ion batteries have been favored by all walks of life due to their high energy density and high specific capacity, relatively low price and cost, and superior cycle performance. They are widely used in new energy vehicles, consumer battery products, military and aerospace fields. However, with the large-scale mining of lithium mines around the world, the price of lithium mines has been rising. More and more people are paying attention to alternative new battery systems, among which sodium-ion batteries have become a hot spot in the future new energy battery market due to their cost and performance advantages.

[0003] There are three main cathode materials in sodium ion batteries: transition metal oxides, Prussian blue analogs, and polyanion materials. Among them, sodium vanadium phosphate (Na3V2(PO4)3) is one of the mainstream materials of the polyanion route. It has good electrochemical performance and high safety, relatively stable material structure, good cycle life, and can maintain excellent electrochemical performance even at high current density. However, the vanadium in sodium vanadium phosphate is expensive. The cathode material cannot be effectively recycled at the end of each battery life, resulting in a large amount of vanadium being wasted, which greatly increases the cost of the enterprise. In addition, metallic vanadium is highly toxic and carcinogenic. If the cathode material of sodium vanadium battery cannot be recycled in time, it will also cause damage to the environment. In addition to vanadium, phosphorus resources in waste sodium ion batteries also have important recycling value. Phosphorus is one of the key elements in the manufacture of battery cathode materials, and it is also an important component of agricultural fertilizers. Phosphorus in waste sodium ion batteries can cause phosphorus pollution. When phosphorus enters the water body, it will cause eutrophication of the water body and destroy the aquatic ecological balance. With the rapid development of new energy vehicles and renewable energy storage systems, the production of waste batteries is increasing, which has prompted the emphasis on battery recycling technologies. These recycling processes can not only bring economic benefits, but also solve the environmental problems caused by the accumulation of waste batteries.

[0004] At present, the industry mainly uses extractants to carry out targeted large-scale recovery of vanadium. For example, the literature "Application Status and Development Trend of P204 Extraction of Vanadium" (DOI: 10.3969 / j.issn.1000-6532.2023.03.011), "Research Progress in Extraction of Vanadium from Vanadium-Containing Acid Leaching Solution" (DOI: 10.13779 / j.cnki.issn1001-0076.2023.07.008), "N235 Supported Liquid Membrane Separation of Shale Vanadium Acid Leaching Solution and Mass Transfer Mechanism" (DOI: 10.11817 / j.ysxb.1004.0609.2020-36484), "Research on Extraction of Vanadium from Stone Coal Acid Leaching Solution with N235" (DOI: 10.7666 / d.D795541), etc., systematically introduces the recovery effect of different extractants on vanadium. However, the above-mentioned extractants (such as P204 and N235) are expensive to use and have a high risk factor. They are physiologically toxic to organisms, and ingestion or exposure to them may lead to growth inhibition, reproduction problems or death. In addition, soil contamination caused by extractants may affect the function and structure of soil microbial communities and have an adverse effect on the stability of the ecosystem. Therefore, a greener and safer recycling process is needed to reduce the pollution of battery recycling to the environment.

[0005] For example, the Chinese invention patent with publication number CN115341098A discloses a method for recovering vanadium from waste sodium ion batteries, comprising the following steps: recovering sodium vanadium phosphate, a cathode material, from waste sodium ion batteries; calcining the sodium vanadium phosphate under an oxygen atmosphere, obtaining a calcined product after the calcination; acid leaching the calcined product, filtering to obtain a leachate after the acid leaching; adjusting the pH of the leachate to 5-7 for vanadium precipitation reaction, collecting solid products after the reaction; drying and calcining the solid products in sequence to obtain vanadium pentoxide. The method provided by the invention can convert vanadium in sodium vanadium phosphate, a cathode material, into vanadium pentoxide, thereby realizing the recycling of vanadium, and the purity of vanadium pentoxide is high and the recovery rate is high. However, the process path has low selectivity for elements without using an extractant. Only vanadium can be recovered by acid leaching with inorganic acid in an aqueous solution environment, and the recycling effect is limited. In addition, some water-soluble compounds are difficult to remove, so that other elements such as phosphorus remain in the product, which restricts the further improvement of purity. In addition, the inorganic acid used in the acid leaching process is selected from sulfuric acid, nitric acid, and hydrochloric acid. In industrial production lines, strong acids will corrode equipment, and all equipment needs to be coated with a layer of polyvinyl chloride (PVC) material, which greatly increases the cost. In addition, in industrial production, strong acids are usually controlled products, and the access to their raw materials also restricts the large-scale application of this process at the industrial level.

[0006] In summary, if the sodium vanadium phosphate cathode material can be recycled, the vanadium and phosphorus therein can be recovered to make electrode materials for other secondary batteries (such as lithium-ion batteries, sodium-ion batteries, aqueous zinc ions, etc.), it can not only further reduce the cost of sodium-ion batteries, but also reduce the harm to workers and the environment. Therefore, it is of great significance to provide an industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode materials. Summary of the invention

[0007] In view of the above-mentioned defects of the prior art, in the first aspect of the present invention, a method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode materials, which is safe, efficient, has a high recycling rate and is suitable for large-scale production, is provided, comprising the following steps: (1) Discharging the discarded sodium ion batteries to make them fully discharged, and then disassembling and recycling them to obtain sodium vanadium phosphate materials; (2) adding the sodium vanadium phosphate material to an oxalic acid aqueous solution for acid leaching, so that the material is completely dissolved in the oxalic acid aqueous solution to obtain a sodium vanadium phosphate acid leaching solution; (3) adding a magnesium chloride aqueous solution to the sodium vanadium phosphate acid leaching solution, adjusting the pH of the system to 9-10 with ammonia water and performing a phosphorus precipitation reaction; after no further precipitation is generated, recovering the generated magnesium ammonium phosphate precipitate and obtaining a dephosphorization solution; (4) adding an aqueous solution of ammonium chloride to the dephosphorization solution to adjust the pH of the system to 6-7 and perform a vanadium precipitation reaction; after no further precipitate is generated, recovering the ammonium metavanadate precipitate; (5) The ammonium metavanadate precipitate is calcined and oxidized in an aerobic environment to obtain vanadium pentoxide.

[0008] When this method is used to recover sodium vanadium phosphate materials from waste sodium ion batteries, the batteries must be fully discharged before proceeding to the subsequent steps. If the batteries cannot be fully discharged, different valence states of vanadium will exist in the sodium vanadium phosphate, such as Na 3-x V 3+ 2-x V 4+ x (PO4)3 and Na 3+x V 3 + 2-x V 2+ x(PO4)3, by-products will be generated in the subsequent impurity removal process. There are two ways to achieve complete discharge in this field: one is physical discharge, which is mainly through external load power consumption, the battery is connected to the resistor, and the power in the battery is consumed by heat release. The other is chemical discharge, that is, using the positive and negative metals of the battery as the cathode and anode, and consuming the residual power in the battery through the electrolysis process in the solution. Physical discharge is currently only suitable for small-scale applications in laboratory environments, and it is difficult to achieve large-scale discharge. Therefore, at the industrial level, chemical discharge is particularly suitable for the treatment method of the present invention. Sodium vanadium phosphate material can be recovered by general operations in this field. First, the waste sodium ion battery treated by discharge is physically disassembled, and the obtained electrode is cleaned and then the split positive electrode sheet is stirred at high speed in an aqueous solution to completely separate the current collector (generally aluminum foil) and the positive electrode material (sodium vanadium phosphate). The fluid is then filtered back to obtain a sodium vanadium phosphate solution, which is centrifuged and the lower layer of precipitation is collected, and the sodium vanadium phosphate material can be obtained after drying.

[0009] Preferably, in step (2), the concentration of the aqueous oxalic acid solution is 1-5 mol / L.

[0010] Preferably, in step (2), the acid leaching treatment temperature is 50-150°C and the treatment time is 2-6 hours.

[0011] The present invention uses magnesium chloride, ammonia water and ammonium chloride with excellent solubility as raw materials for phosphorus precipitation reaction and vanadium precipitation reaction. Since the content of sodium vanadium phosphate in discarded sodium ion batteries varies, those skilled in the art can select the appropriate amount of magnesium chloride aqueous solution, ammonia water and ammonium chloride aqueous solution to be added according to the actual source of discarded sodium ion batteries. The above raw materials have good reactivity with phosphorus and vanadium. With the addition of reactants, the precipitate required for the reaction can be obtained at room temperature. Therefore, when no further precipitate is generated, it can be regarded that the recovery of the target element has been completed, and this effect can be achieved by processing for 4-6 hours in actual production.

[0012] Preferably, in step (3), the concentration of the magnesium chloride aqueous solution is 1-3 mol / L, and the concentration of the ammonia water is 0.5-2 mol / L.

[0013] Preferably, in step (3), the phosphorus precipitation reaction is carried out at room temperature and the reaction time is 4-6 h.

[0014] Preferably, in step (4), the concentration of the aqueous ammonium chloride solution is 1-3 mol / L.

[0015] Preferably, in step (4), the vanadium precipitation reaction is carried out at room temperature, and the reaction time is 4-6 h.

[0016] The introduction of oxygen during calcination helps to ensure that the vanadium in the decomposition process of ammonium metavanadate is completely oxidized, thereby increasing the purity of vanadium pentoxide and giving it good electrochemical properties and stability as a positive electrode material in other new energy batteries.

[0017] Preferably, in step (5), the calcination temperature is 400-550° C., the calcination time is 6-7.5 h, and the oxygen flow rate during the calcination process is 3-6 L / min.

[0018] The increase in the types of target elements to be recovered will pose a challenge to the separation of products, so the existing processes in this field usually only focus on achieving the recycling and reuse of a single target element. In the present invention, in addition to vanadium, the recovery of phosphorus not only improves the utilization value of waste sodium-ion batteries, but is also necessary in controlling the quality of products. According to the needs of industrial-grade production, the inventors have found that the presence of phosphorus will deteriorate the quality of the vanadium pentoxide product. Phosphorus may cause impurities or impure substances to be produced during the recovery of vanadium pentoxide, thereby reducing the purity of vanadium pentoxide. This will affect the specific capacity and cyclability of vanadium pentoxide as an electrode material for other batteries; in some specific applications, it will also affect its performance or stability, thereby reducing the quality or reliability of the product. At the same time, the presence of phosphorus may have an adverse effect on the production process of vanadium pentoxide, requiring additional processing steps to remove phosphorus or treat reaction products caused by phosphorus, increasing production costs and complexity.

[0019] Based on the above technical scheme, the concept and principle of the present invention is that, without using an extractant, magnesium chloride and ammonia water are added before vanadium precipitation, and phosphorus precipitation operation is introduced to recover the precipitate in the form of magnesium ammonium phosphate, thereby optimizing the adverse effect of phosphorus on vanadium recovery. The inventors have used a method to generate magnesium ammonium phosphate (Mg 2+ + NH4 + + PO4 3- → MgNH4PO4) to remove phosphorus. This step is designed based on its poor water solubility, easy separation and multi-faceted uses. Magnesium ammonium phosphate is widely used as a feed and fertilizer additive, and is also used in medicine. It can also be used in the manufacture of coatings, carbamates, and soft foam flame retardants. Magnesium ammonium phosphate has been listed as a fertilizer abroad and is used as a long-term inorganic nitrogen fertilizer for fruit trees, lawns, flowers, etc. Recycling phosphorus is necessary to reduce waste and improve the process. By recycling phosphorus, the adverse effects of phosphorus on the vanadium pentoxide recovery process (NH4VO3+ O2→ V2O5 + H2O +NH3) can be avoided, ensuring that the produced vanadium pentoxide has high purity and good performance. This helps to improve the efficiency of the process and product quality, while reducing the waste of raw materials. This step fully considers the difficulty of separating phosphorus and the use of the product, and has good industrial application potential.

[0020] Cost control is the most important item for industrial-grade industrialization. In the acid leaching process of this method, organic weak acid oxalic acid is used instead of inorganic strong acids, such as sulfuric acid, hydrochloric acid, nitric acid, etc. For industrialization, the loss of equipment to oxalic acid is much less than that of strong acid. Secondly, oxalic acid itself has good safety, low adverse effects on the environment, and it is not a controlled product, which is conducive to the promotion of industrialization in enterprise production. As mentioned above, in the subsequent precipitation process of magnesium ammonium phosphate, ammonia water needs to be added to simultaneously adjust the pH of the solution. If an inorganic strong acid is used, the amount of ammonia water required is large, which will increase the recovery cost. Therefore, the choice of oxalic acid not only takes into account the treatment effect and cost of acid leaching, but also takes into account the amount of raw materials used in subsequent operations, thereby achieving the purpose of reducing costs.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects: The invention provides an industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode materials. The recovery process of the method has the advantages of safety, high efficiency, high recovery rate and suitability for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a flow chart of the industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material of Example 1; Figure 2 This is a physical photo of the vanadium pentoxide recovered in Example 1; Figure 3 is an X-ray diffraction (XRD) pattern of vanadium pentoxide recovered in Example 1; Figure 4 This is a cycle performance diagram of the vanadium pentoxide recovered in Example 1-4 when used in an aqueous zinc ion battery. DETAILED DESCRIPTION

[0023] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0024] In the following embodiments: Oxalic acid, concentration: 99.6 wt.%; magnesium chloride, purity: 99 wt.%; ammonium chloride, purity: 99 wt.%.

[0025] Example 1 Industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode materials, such as Figure 1 As shown, the steps are as follows: (1) The recycled waste sodium ion batteries are discharged to make them fully discharged, and then they are physically separated into a positive electrode containing positive electrode materials, an electrolyte, a separator and a negative electrode containing negative electrode materials; the positive electrode is collected and the rest is recycled uniformly, the positive electrode is ultrasonically cleaned with deionized water at room temperature for 2 h, and then the positive electrode sheet is stirred at a high speed of 1200 rpm in an aqueous solution for 2 h to completely separate the aluminum foil from the sodium vanadium phosphate, and the waste aluminum foil is filtered and collected and sent to an aluminum plant for recycling to reduce costs; the filtrate is centrifuged at a rate of 6000 rpm for 5 times, each time for 2 min, the lower precipitate is collected, and it is dried at 60 ° C for 12 h to obtain the sodium vanadium phosphate material; (2) preparing oxalic acid into a 2 mol / L oxalic acid aqueous solution, adding sodium vanadium phosphate material to the oxalic acid aqueous solution for acid leaching, stirring at 50 °C for 2 h, then cooling to room temperature, adding an appropriate amount of distilled water to dilute the solution so that the sodium vanadium phosphate material is completely dissolved, and obtaining a sodium vanadium phosphate acid leaching solution; (3) Magnesium chloride is prepared into a 1 mol / L magnesium chloride aqueous solution, and the magnesium chloride aqueous solution is added to the sodium vanadium phosphate acid leaching solution, and the pH is adjusted to a range of 9-10 using 0.5 mol / L ammonia water, and phosphorus precipitation reaction is carried out at room temperature for 6 hours; after the reaction is completed, the magnesium ammonium phosphate precipitate and the dephosphorization solution are obtained by filtration; the magnesium ammonium phosphate precipitate is dried at 60 °C for 6 hours to complete the recovery of phosphorus; (4) preparing ammonium chloride into a 3 mol / L ammonium chloride aqueous solution, adding the ammonium chloride aqueous solution to the dephosphorization solution and controlling the pH value to be in the range of 6-7, and performing vanadium precipitation reaction at room temperature for 6 hours; after the reaction is completed, filtering to obtain ammonium metavanadate precipitate, and drying it at 60°C for 8 hours; (5) The ammonium metavanadate precipitate was calcined at 550 °C for 6 h under oxygen conditions to completely oxidize the vanadium. The oxygen flow rate during the calcination process was 3 L / min, and solid powdered vanadium pentoxide was obtained. The actual photo is shown in Figure 2 shown.

[0026] The obtained vanadium pentoxide was characterized by XRD. Figure 3 shown. Figure 3 The characteristic peaks indicate that the target product is recovered, and the process of the present invention has good application prospects.

[0027] Example 2 The industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode materials comprises the following steps: (1) The recycled waste sodium ion batteries are discharged to make them fully discharged, and then they are physically separated into a positive electrode containing positive electrode materials, an electrolyte, a separator and a negative electrode containing negative electrode materials; the positive electrode is collected and the rest is recycled uniformly, the positive electrode is ultrasonically cleaned with deionized water at room temperature for 2 h, and then the positive electrode sheet is stirred at a high speed of 1200 rpm in an aqueous solution for 2 h to completely separate the aluminum foil from the sodium vanadium phosphate, and the waste aluminum foil is filtered and collected and sent to an aluminum plant for recycling to reduce costs; the filtrate is centrifuged at a rate of 6000 rpm for 5 times, each time for 2 min, the lower precipitate is collected, and it is dried at 60 ° C for 12 h to obtain the sodium vanadium phosphate material; (2) preparing oxalic acid into a 3 mol / L oxalic acid aqueous solution, adding sodium vanadium phosphate material to the oxalic acid aqueous solution for acid leaching, stirring at 75 °C for 2 h, then cooling to room temperature, adding an appropriate amount of distilled water to dilute the solution so that the sodium vanadium phosphate material is completely dissolved, and obtaining a sodium vanadium phosphate acid leaching solution; (3) Magnesium chloride is prepared into a 1.5 mol / L magnesium chloride aqueous solution, and the magnesium chloride aqueous solution is added to the sodium vanadium phosphate acid leaching solution. The pH is adjusted to a range of 9-10 using 1 mol / L ammonia water, and phosphorus precipitation is carried out at room temperature for 6 hours. After the reaction is completed, the magnesium ammonium phosphate precipitate and the dephosphorization solution are obtained by filtration. The magnesium ammonium phosphate precipitate is dried at 60 °C for 6 hours to complete the recovery of phosphorus. (4) preparing ammonium chloride into a 3 mol / L ammonium chloride aqueous solution, adding the ammonium chloride aqueous solution to the dephosphorization solution and controlling the pH value to be in the range of 6-7, and performing vanadium precipitation reaction at room temperature for 6 hours; after the reaction is completed, filtering to obtain ammonium metavanadate precipitate, and drying it at 60°C for 8 hours; (5) The ammonium metavanadate precipitate was calcined at 500 °C for 6.5 h under oxygen conditions to completely oxidize the vanadium. The oxygen flow rate during the calcination process was 4 L / min, and solid powdered vanadium pentoxide was obtained.

[0028] Example 3 The industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode materials comprises the following steps: (1) The recycled waste sodium ion batteries are discharged to make them fully discharged, and then they are physically separated into a positive electrode containing positive electrode materials, an electrolyte, a separator and a negative electrode containing negative electrode materials; the positive electrode is collected and the rest is recycled uniformly, the positive electrode is ultrasonically cleaned with deionized water at room temperature for 2 h, and then the positive electrode sheet is stirred at a high speed of 1200 rpm in an aqueous solution for 2 h to completely separate the aluminum foil from the sodium vanadium phosphate, and the waste aluminum foil is filtered and collected and sent to an aluminum plant for recycling to reduce costs; the filtrate is centrifuged at a rate of 6000 rpm for 5 times, each time for 2 min, the lower precipitate is collected, and it is dried at 60 ° C for 12 h to obtain the sodium vanadium phosphate material; (2) preparing oxalic acid into a 4 mol / L oxalic acid aqueous solution, adding sodium vanadium phosphate material to the oxalic acid aqueous solution for acid leaching treatment, stirring at 100 °C for 2 h, then cooling to room temperature, adding an appropriate amount of distilled water to dilute the solution so that the sodium vanadium phosphate material is completely dissolved, and obtaining a sodium vanadium phosphate acid leaching solution; (3) Magnesium chloride is prepared into a 2 mol / L magnesium chloride aqueous solution, and the magnesium chloride aqueous solution is added to the sodium vanadium phosphate acid leaching solution, and the pH is adjusted to a range of 9-10 using 1.5 mol / L ammonia water, and phosphorus precipitation reaction is carried out at room temperature for 6 hours; after the reaction is completed, the magnesium ammonium phosphate precipitate and the dephosphorization solution are obtained by filtration; the magnesium ammonium phosphate precipitate is dried at 60 °C for 6 hours to complete the recovery of phosphorus; (4) preparing ammonium chloride into a 3 mol / L ammonium chloride aqueous solution, adding the ammonium chloride aqueous solution to the dephosphorization solution and controlling the pH value to be in the range of 6-7, and performing vanadium precipitation reaction at room temperature for 6 hours; after the reaction is completed, filtering to obtain ammonium metavanadate precipitate, and drying it at 60°C for 8 hours; (5) The ammonium metavanadate precipitate was calcined at 450 °C for 7 h in an oxygen-filled condition to completely oxidize the vanadium. The oxygen flow rate during the calcination process was 5 L / min, and solid powdered vanadium pentoxide was obtained.

[0029] Example 4 The industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode materials comprises the following steps: (1) The recycled waste sodium ion batteries are discharged to make them fully discharged, and then they are physically separated into a positive electrode containing positive electrode materials, an electrolyte, a separator and a negative electrode containing negative electrode materials; the positive electrode is collected and the rest is recycled uniformly, the positive electrode is ultrasonically cleaned with deionized water at room temperature for 2 h, and then the positive electrode sheet is stirred at a high speed of 1200 rpm in an aqueous solution for 2 h to completely separate the aluminum foil from the sodium vanadium phosphate, and the waste aluminum foil is filtered and collected and sent to an aluminum plant for recycling to reduce costs; the filtrate is centrifuged at a rate of 6000 rpm for 5 times, each time for 2 min, the lower precipitate is collected, and it is dried at 60 ° C for 12 h to obtain the sodium vanadium phosphate material; (2) preparing oxalic acid into a 5 mol / L oxalic acid aqueous solution, adding sodium vanadium phosphate material to the oxalic acid aqueous solution for acid leaching, stirring at 125 °C for 2 h, then cooling to room temperature, adding an appropriate amount of distilled water to dilute the solution, so that the sodium vanadium phosphate material is completely dissolved, and obtaining a sodium vanadium phosphate acid leaching solution; (3) Magnesium chloride is prepared into a 2.5 mol / L magnesium chloride aqueous solution, and the magnesium chloride aqueous solution is added to the sodium vanadium phosphate acid leaching solution. The pH is adjusted to a range of 9-10 using 2 mol / L ammonia water, and phosphorus precipitation reaction is carried out at room temperature for 6 hours; after the reaction is completed, the magnesium ammonium phosphate precipitate and the dephosphorization solution are obtained by filtration; the magnesium ammonium phosphate precipitate is dried at 60 °C for 6 hours to complete the recovery of phosphorus; (4) preparing ammonium chloride into a 2.5 mol / L ammonium chloride aqueous solution, adding the ammonium chloride aqueous solution to the dephosphorization solution and controlling the pH value to be in the range of 6-7, and performing vanadium precipitation reaction at room temperature for 6 h; after the reaction is completed, filtering to obtain ammonium metavanadate precipitate, and drying it at 60 °C for 8 h; (5) The ammonium metavanadate precipitate was calcined at 400 °C for 7.5 h under oxygen conditions to completely oxidize the vanadium. The oxygen flow rate during the calcination process was 6 L / min, and solid powdered vanadium pentoxide was obtained.

[0030] Example 5 In this embodiment, the vanadium pentoxide recovered from the waste sodium ion battery in Examples 1-4 is used to make an aqueous zinc ion battery. The recovered vanadium pentoxide and carbon black and polyvinylidene fluoride (PVDF) with a concentration of 0.05 g / mL are mixed in a mass ratio of 7:2:1, and a slurry is prepared with 1-methyl-2-pyrrolidone (NMP) liquid as a solvent. A carbon cloth is used as a current collector, and the prepared slurry is evenly applied on the current collector. The positive electrode of the aqueous zinc ion battery is obtained by drying at 60 ° C for 12 h. Zinc foil is then used as the negative electrode, and a button-type aqueous zinc ion battery is assembled with a CR2032 battery shell.

[0031] The cycle performance of each group was tested using a common method in the art. The test was carried out at room temperature. The cycle performance test results of the aqueous zinc ion battery corresponding to Examples 1-4 are shown in Figure 4 As shown, the test results of specific capacity after 100 cycles in the test are shown in Table 1.

[0032] Table 1: Test results of specific capacity of aqueous zinc-ion batteries after 100 cycles

[0033] Depend on Figure 4 It can be seen from the test results in Table 1 that the vanadium pentoxide recovered by the present invention has good cycle performance and high coulombic efficiency due to low impurities and high purity for use in secondary batteries. Among them, the vanadium pentoxide in Example 1 has the best performance in application, and its specific capacity after 100 cycles can reach 200.90 mAh / g.

[0034] In summary, the present invention adds magnesium chloride and ammonia water before vanadium precipitation without using an extractant, introduces a phosphorus precipitation operation to recover the precipitate in the form of magnesium ammonium phosphate, and optimizes the adverse effect of phosphorus on the recovery of vanadium. Phosphorus is removed in the process by generating magnesium ammonium phosphate. This step is designed based on its poor water solubility, easy separation and various uses. The obtained magnesium ammonium phosphate can be widely used in various fields. By recovering phosphorus, the adverse effect of phosphorus on the vanadium pentoxide recovery process can be avoided, ensuring that the produced vanadium pentoxide has high purity and good performance, which helps to improve the efficiency of the process and product quality, while reducing the waste of raw materials. This step fully considers the difficulty of separating the phosphorus element and the use of the product, and the recovered vanadium pentoxide is made into other secondary batteries, which can not only further reduce the cost of sodium ion batteries, etc., but also reduce harm to workers and the environment, and has good industrial application potential.

[0035] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. An industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material, characterized in that: The steps include: (1) Discharging the discarded sodium ion batteries to make them fully discharged, and then disassembling and recycling them to obtain sodium vanadium phosphate materials; (2) adding the sodium vanadium phosphate material to an oxalic acid aqueous solution for acid leaching, so that the material is completely dissolved in the oxalic acid aqueous solution to obtain a sodium vanadium phosphate acid leaching solution; (3) adding a magnesium chloride aqueous solution to the sodium vanadium phosphate acid leaching solution, adjusting the pH of the system to 9-10 with ammonia water, and performing a phosphorus precipitation reaction; After no further precipitation is generated, recovering the generated magnesium ammonium phosphate precipitate and obtaining a dephosphorization solution; (4) adding an aqueous solution of ammonium chloride to the dephosphorization solution to adjust the pH of the system to 6-7 and perform a vanadium precipitation reaction; after no further precipitate is generated, recovering the ammonium metavanadate precipitate; (5) The ammonium metavanadate precipitate is calcined and oxidized in an aerobic environment to obtain vanadium pentoxide.

2. The method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material at an industrial level according to claim 1, characterized in that: In the step (2), the concentration of the oxalic acid aqueous solution is 1-5 mol / L.

3. The method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material at an industrial level according to claim 1, characterized in that: In the step (2), the acid leaching treatment temperature is 50-150°C and the treatment time is 2-6 hours.

4. The method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material at an industrial level according to claim 1, characterized in that: In the step (3), the concentration of the magnesium chloride aqueous solution is 1-3 mol / L, and the concentration of the ammonia water is 0.5-2 mol / L.

5. The industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode material according to claim 1, characterized in that: In the step (3), the phosphorus precipitation reaction is carried out at room temperature and the reaction time is 4-6 hours.

6. The industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material according to claim 1, characterized in that: In the step (4), the concentration of the aqueous ammonium chloride solution is 1-3 mol / L.

7. The industrial-grade method for recovering vanadium and phosphorus from waste sodium vanadium phosphate positive electrode material according to claim 1, characterized in that: In the step (4), the vanadium precipitation reaction is carried out at room temperature and the reaction time is 4-6 h.

8. The method for recovering vanadium and phosphorus from waste sodium vanadium phosphate cathode material at an industrial level according to claim 1, characterized in that: In the step (5), the calcination temperature is 400-550°C, the calcination time is 6-7.5 h, and the oxygen flow rate during the calcination process is 3-6 L / min.

Citation Information

Patent Citations

  • Method for recovering vanadium from waste sodium-ion battery

    CN115341098A

Cited By

  • Method for preparing vanadium electrolyte from waste vanadium-based battery positive electrode material

    CN121790574A

  • Method for recovering vanadium metal from zinc-ion batteries

    TWI929954B