Leaching method of sulfur-containing siliceous mudstone type uranium ore

By employing crushing, piling, wetting, acid pre-leaching, and microbial leaching steps, and utilizing acidophilic iron-oxidizing bacteria and sulfur-oxidizing bacteria to oxidize pyrite, the problems of low uranium leaching rate and high production cost in existing technologies have been solved, achieving efficient uranium leaching and cost reduction.

CN118910438APending Publication Date: 2024-11-08BEIJING RESEARCH INSTITUTE OF CHEMICAL ENGINEERING AND METALLURGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410986422.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing bioleaching process of sulfur-bearing siliceous mudstone-type uranium ore, microorganisms have difficulty efficiently oxidizing and decomposing pyrite, resulting in low uranium leaching rate, high sulfuric acid consumption, high production cost, and significant construction and maintenance costs for biological contact oxidation tanks.

Method used

The process involves crushing, piling, wetting, acid pre-leaching, microbial leaching, and subsequent sulfuric acid leaching. It utilizes acidophilic iron-oxidizing bacteria and sulfur-oxidizing bacteria to oxidize pyrite, producing sulfuric acid and adsorbing the tailings. This eliminates the need for a biological contact oxidation tank and allows for direct spraying of the microbial leaching agent, thus optimizing the process flow.

Benefits of technology

This improved the uranium leaching rate, reduced the amount of sulfuric acid used and the acidity of the leaching solution, simplified the process, and lowered production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a leaching method of sulfur-containing siliceous mudstone type uranium ore. Aiming at the problems of high leaching reagent consumption, high residual acid in leachate, high production cost and the like caused by high pyrite content and close relationship with uranium in the sulfur-containing siliceous mudstone type uranium ore, the method disclosed by the invention has the advantages that the pyrite wrapping uranium ore is oxidized and decomposed through iron-sulfur oxidizing bacteria, the uranium ore is exposed, the leaching rate of uranium is effectively improved, and the leaching efficiency of uranium is improved. The consumption of a leaching reagent and the residual acid of a leaching solution are reduced, meanwhile, the leaching technological process is simplified, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of uranium ore biological leaching, and in particular relates to a method for biologically leaching uranium from siliceous mudstone-type uranium ore containing sulfide pyrite. Background Art

[0002] Pyrite is one of the most common sulfide minerals, often associated with rare non-ferrous and radioactive metal minerals. The main rock-forming minerals of sulfur-bearing siliceous mudstone-type uranium deposits are quartz and illite. The content of sulfide pyrite in the ore is usually high, generally around 5%, and can reach more than 10% in some areas. Uranium minerals in the ore are often wrapped by pyrite. In order to fully leach the uranium in the ore and improve the uranium leaching rate, the pyrite wrapped in the uranium minerals needs to be oxidized and decomposed.

[0003] This type of ore has a low carbonate content and a very low basic acid consumption of only about 1%. When acid leaching is used, in order to reduce the uranium content of the leaching tailings to below 0.02%, the amount of sulfuric acid must be increased to decompose the pyrite. The amount of stirred leaching acid is 6% to 8%, and the residual acid in the leachate is high. The sulfuric acid concentration in the leachate is nearly 40g / L to 60g / L. Because the strong alkaline anion exchange resin used in the subsequent ion exchange adsorption of the leaching is sensitive to HSO4 in the solution. - With the increase of sulfuric acid concentration in the leaching solution, HSO4 - Increase, reduce the energy with UO2 2+ SO4 forming anionic complex 2- , resulting in a significant decrease in the resin uranium adsorption capacity.

[0004] Bioleaching technology can be used for sulfur-containing uranium ores, using leaching microorganisms to oxidize and adsorb sulfides in tailings or ores to produce Fe 3+ and sulfuric acid to leach uranium from the ore. At present, the basic process flow of uranium ore biological leaching is ore crushing - heap building - sulfuric acid acid leaching uranium - bacterial oxidation leaching uranium - unloading the heap, in which bacterial oxidation leaching of uranium is to spray the prepared bacterial oxidant into the ore after acid leaching for bacterial oxidation leaching of uranium. The bacterial oxidant is prepared by adsorbing the tail liquid through a biological contact oxidation tank. The main problems of this process flow are: (1) The leaching microorganisms are adsorbed on the filler of the biological contact oxidation tank, and the microorganisms cannot efficiently oxidize the sulfide in the ore, cannot break the sulfide's coating on the uranium, and have little effect on reducing the consumption of sulfuric acid reagent for leaching; (2) The biological contact oxidation tank for preparing bacterial oxidants requires a large amount of manpower, material and financial resources during the construction, operation and maintenance process. For example, a certain amount of funds are required for the construction of the oxidation tank, the corrosion protection of the tank body, the installation of aeration pipes and fillers, and the operation of the fan, which makes the production cost high.

[0005] Patent 201610299804 also involves a solution for bioleaching of sulfur-containing uranium ores, but has many defects. The present invention conducts in-depth research on this basis and further improves some problems existing in the patent.

[0006] The difference between the present invention and Patent 201610299804 is that the properties of the ore are different. The present invention is aimed at siliceous mudstone uranium ore with high pyrite content in the ore, while Patent 201610299804 is aimed at uranium ore with high organic matter and iron content in the ore. In the present invention, the pyrite content of the ore is relatively high, reaching 6%, and the sulfur content is 3.2% (the sulfur content is 2.7 times that of Example 2 in the 201610299804 document), and pyrite is closely related to uranium. There are two examples in the patent 201610299804 document. In Example 1, the organic carbon content in the ore is 12.57%, and the proportions of Fe2O3 and FeO are 3.94% and 0.252% respectively. Example 1 does not mention the sulfur content, and it is speculated that the sulfur content in the ore is low; in Example 2, the organic carbon content in the ore is 13.10%, and the proportions of Fe2O3 and FeO are 4.00% and 0.236% respectively, and the sulfur content is 1.18%; the ore properties of this patent are that the organic matter and iron content in the ore are high, and the sulfur content is not high. Second, the role of microorganisms is different. The microorganisms of the present invention oxidize and crack the sulfide encapsulating uranium, and at the same time oxidize the ferrous iron in the adsorbed tail liquid into trivalent iron, and the trivalent iron oxidizes the tetravalent uranium in the ore. In the patent 201610299804 document

[0030] , it is clearly stated that bacterial oxidation leaching of uranium is carried out, and the purpose is to oxidize the difficult-to-leach tetravalent uranium in the ore by bacterial ferric sulfate oxidant, and strengthen the leaching of uranium. Third, the process flow is different. When the acidification period of the ore pile ends and the pH of the leaching solution flowing out of the ore pile is less than 2.0, the present invention sprays a leaching agent containing microorganisms to leach the uranium ore. The present invention does not require a biological contact oxidation tank, but directly sprays a leaching agent containing microorganisms. The patent 201610299804 document uses a biological contact oxidation tank, which appears many times in the schematic diagram on the right side of the abstract of the document and in the document. Summary of the invention

[0007] The object of the present invention is to provide a leaching method for sulfur-containing siliceous mudstone-type uranium ore, which can effectively oxidize and decompose pyrite encapsulating uranium minerals, so that the uranium encapsulated therein can be efficiently leached, the uranium leaching rate can be improved, and the amount of sulfuric acid used in the leaching process can be reduced, so that the residual acid in the leaching solution is low, which is beneficial to the subsequent ion exchange adsorption process, and at the same time, the biological contact oxidation tank is omitted, the process is simplified, and the production cost is reduced.

[0008] A leaching method for sulfur-containing siliceous mudstone-type uranium ore comprises the following steps:

[0009] (1) crushing sulfur-containing siliceous mudstone-type uranium ore;

[0010] (2) piling the sulfur-containing siliceous uranium ore crushed in step (1);

[0011] (3) wetting the pile built in step (2) with water;

[0012] (4) acid preleaching the ore using a sulfuric acid solution;

[0013] (5) After the acid pre-leaching is completed, the ore is sprayed with a leaching agent containing microorganisms to perform microbial leaching;

[0014] (6) After the microorganisms are leached out, continue to use a solution containing sulfuric acid for spraying acid leaching;

[0015] (7) Extracting uranium by ion exchange from the leaching solution obtained in steps (4), (5), and (6).

[0016] The pyrite content of the sulfur-containing siliceous mudstone-type uranium ore in step (1) is greater than 5%.

[0017] Step (1) crushing the sulfur-containing siliceous mudstone-type uranium ore to an ore particle size of -5 mm.

[0018] The concentration of the sulfuric acid solution used in step (4) is 5-10 g / L; the dosage is 5%-30% of the mass of the ore. When the pH of the leaching solution to be discharged is less than 2.0, the spraying of the sulfuric acid solution is stopped.

[0019] In step (5), when the pH of the leaching solution flowing out of the ore pile in step (4) is less than 2.0, the adsorption tail liquid containing microorganisms is sprayed as a leaching agent, the sulfuric acid concentration in the leaching agent is 2-5 g / L, and the number of bacteria is not less than 1×10 7 The content of bacterial liquid in the logarithmic growth phase is 5% to 30% per ml; the spraying time is 3 to 7 days; the spraying leaching agent is 10% to 25% of the ore mass, and the daily leaching agent spraying time and stop time are 2:1.

[0020] The microorganisms include: acidophilic iron-oxidizing bacteria and sulfur-oxidizing bacteria, such as at least two of Thiobacillus ferrooxidans, Thiobacillus thiooxidans, and Microspirillum ferrooxidans;

[0021] The bacterial colony is inoculated into the adsorption tail liquid of step (7) at a ratio of 5% to 30% for acclimatization and culture at a temperature of 20 to 35°C and a pH of 1.5 to 2.0 until the bacterial solution concentration reaches 1.0×10 7 / mL or more, the redox potential is not less than 470mV, and the culture is acclimated for 3 to 5 times.

[0022] In step (6), a solution containing sulfuric acid is used as a leaching agent to continue spray leaching the ore pile, and the concentration of sulfuric acid in the leaching agent is 2 to 5 g / L.

[0023] In step (6), water or adsorption tail liquid and sulfuric acid are used to prepare a leaching agent.

[0024] Step (6) When the concentration of the leaching solution U flowing out of the ore pile is less than 20 mg / L, water is used for washing and unloading.

[0025] Beneficial effects of the present invention:

[0026] (1) Effectively oxidize and decompose pyrite that encapsulates uranium minerals, allowing the uranium encapsulated therein to be efficiently leached, thereby increasing the uranium leaching rate; (2) Microbial oxidation of pyrite produces sulfuric acid, reducing the consumption of leaching reagents; (3) Reducing the residual acid in the leaching solution is beneficial to the subsequent ion exchange adsorption process; (4) No biological contact oxidation tank is required, simplifying the process and reducing production costs. DETAILED DESCRIPTION

[0027] The following examples are intended to further illustrate the present invention, but are not intended to limit the present invention.

[0028] Comparative Example 1

[0029] The sulfur-containing siliceous mudstone uranium ore used in the experiment has a uranium grade of 0.094% and a pyrite content of 6%. Column leaching simulated heap leaching was used in the laboratory to extract uranium from the uranium ore. The specific steps are as follows:

[0030] (1) crushing the uranium ore to a particle size of -3 mm;

[0031] (2) packing the crushed uranium ore in step (1) into a column with a diameter of 100 mm and a height of 1.7 m;

[0032] (3) wetting the ore pillar obtained in step (2) with clean water;

[0033] (4) During the leaching acidification period, clean water and sulfuric acid are used to prepare the leaching agent, and the sulfuric acid concentration in the leaching agent is 10g / L; the leaching agent sprayed every day is 10% of the ore amount, and the daily leaching stop time ratio is 2:1.

[0034] (5) When the pH of the leaching solution flowing out of the ore pile is less than 2.0, the adsorption tail liquid and sulfuric acid are used to prepare the leaching agent, and the heap leaching spray operation is carried out. The sulfuric acid concentration in the leaching agent is 7g / L, the leaching agent sprayed every day is 10% of the ore amount, and the daily leaching stop time ratio is 2:1;

[0035] (6) When the U concentration of the leaching solution flowing out of the ore pile is less than 20 mg / L, wash the pile with clean water for 1 day, unload the pile, take the tailings, and analyze the uranium content of the tailings;

[0036] (7) Extracting uranium by ion exchange from the leaching solution obtained in steps (4) and (5).

[0037] The results show that after leaching for 60 days, the uranium content of the tailings is 0.024%, the uranium leaching rate based on the slag is 74.5%, the amount of sulfuric acid used is 4.25% of the ore mass, and the residual acid in the leaching solution is 4-6g / L.

[0038] Comparative Example 2 Comparative Example of Biological Oxidation Tank

[0039] The sulfur-containing siliceous mudstone uranium ore used in the experiment has a uranium grade of 0.094% and a pyrite content of 6%. Column leaching simulated heap leaching was used in the laboratory to extract uranium from the uranium ore. The specific steps are as follows:

[0040] (1) crushing the sulfur-containing siliceous uranium ore to an ore particle size of -3 mm;

[0041] (2) packing the crushed uranium ore in step (1) into a column with a diameter of 100 mm and a height of 1.7 m;

[0042] (3) wetting the ore pillar obtained in step (2) with clean water;

[0043] (4) During the leaching acidification period, clean water and sulfuric acid are used to prepare the leaching reagent, the sulfuric acid concentration is 10g / L, the leaching agent sprayed every day is 10% of the ore amount, and the daily leaching stop time ratio is 2:1;

[0044] (5) When the pH of the leachate flowing out of the ore pile is less than 2.0, the bacterial high-iron leaching agent oxidized by the biological contact oxidation tank is sprayed (according to the bacterial liquid culture method in Patent 201610299804, the bacterial species is the same as in Example 1) about g / L, the sulfuric acid concentration is 5g / L, the daily spraying amount is 10% of the ore amount, and the daily leaching stop time ratio is 2:1;

[0045] (6) When the redox potential Eh value of the adsorption tail liquid obtained by ion exchange of the leaching solution in step (5) is greater than 500 mV, the adsorption tail liquid and sulfuric acid are used to prepare a leaching agent for spraying the ore, the sulfuric acid concentration is 4 g / L, the daily spraying amount is 10% of the ore amount, and the daily leaching stop time ratio is 2:1;

[0046] (7) When the U concentration of the leaching solution flowing out of the ore pile is less than 20 mg / L, wash the pile with clean water for 1 day, unload the pile, take the tailings, and analyze the uranium content of the tailings;

[0047] (8) performing ion exchange on the leaching solution obtained in steps (4), (5), and (6), wherein the adsorption tail liquid in steps (4), (5) enters a biological contact oxidation tank for oxidation regeneration.

[0048] The results show that after leaching for 45 days, the uranium content of the tailings is 0.022%, the uranium leaching rate based on the slag is 76.6%, the amount of sulfuric acid used is 2.15% of the ore mass, and the residual acid in the leaching solution is 2-3 g / L.

[0049] Example 1

[0050] The sulfur-containing siliceous mudstone uranium ore used in the experiment has a uranium grade of 0.094% and a pyrite content of 6%. Column leaching simulated heap leaching was used in the laboratory to extract uranium from the uranium ore. The specific steps are as follows:

[0051] (1) crushing the sulfur-containing siliceous uranium ore to an ore particle size of -3 mm;

[0052] (2) packing the crushed uranium ore in step (1) into a column with a diameter of 100 mm and a height of 1.7 m;

[0053] (3) wetting the ore pillar obtained in step (2) with clean water;

[0054] (4) During the leaching acidification period, clean water and sulfuric acid are used to prepare the leaching reagent, and the sulfuric acid concentration is 10g / L; the leaching agent sprayed every day is 10% of the ore amount; the daily leaching stop time ratio is 2:1;

[0055] (5) When the pH of the leaching solution flowing out of the ore pile is less than 2.0, the adsorption tail liquid containing microorganisms is sprayed as the leaching agent. The spraying time is 5 days, the bacterial liquid content in the leaching agent is 15%, and the number of bacteria in the bacterial liquid is about 1×10 7 / ml, the concentration of sulfuric acid of the leaching agent is 4g / L; the leaching agent sprayed every day is 10% of the ore amount; the daily leaching stop time ratio is 2:1;

[0056] (6) After step (5) is completed, the adsorption tail liquid and sulfuric acid are used to prepare a leaching agent, the sulfuric acid concentration is 4g / L, and a heap leaching spray operation is performed; the leaching agent sprayed every day is 10% of the ore amount, and the leaching stop time ratio is 2:1;

[0057] (7) When the U concentration of the leaching solution flowing out of the ore pile is less than 20 mg / L, wash the pile with clean water for 1 day, unload the pile, take the tailings, and analyze the uranium content of the tailings;

[0058] (8) Extracting uranium by ion exchange from the leaching solution obtained in steps (4), (5), and (6).

[0059] The results show that after leaching for 45 days, the uranium content of the tailings is 0.017%, the uranium leaching rate based on the slag is 81.9%, the amount of sulfuric acid used is 1.85% of the ore mass, and the residual acid in the leaching solution is 1-3 g / L.

[0060] The microorganism acclimation process of the extractant containing microorganisms of the present invention is as follows: a mixed bacteria of Thiobacillus ferrooxidans and Thiobacillus thiooxidans (the two bacteria are in a ratio of 1:1) is inoculated into the adsorption tail liquid after ion exchange at a ratio of 20% for acclimation and cultivation, the cultivation temperature is 30°C, the pH is 2.0, and the culture is carried out until the bacterial solution concentration reaches 1.0×10 7 / mL or more, the redox potential is greater than 500mV, and the culture is acclimated for 3 times.

[0061] Example 2 Condition Exploration

[0062] Test use A total of 3 columns were used for comparative tests. The ore volume was 20 kg, the spray volume was 10%, and the spray-stop ratio was 2:1. The ore particle sizes were -8 mm, -5 mm, and -3 mm. First, clean water was sprayed, and then 10 g / L sulfuric acid solution was sprayed. When the pH of the leaching solution was <2.0, a leaching agent containing mixed bacteria was sprayed. The spraying time was 5 days, the bacterial liquid content in the leaching agent was 15%, and the number of bacteria was about 1×10 7 / ml, the concentration of sulfuric acid of the leaching agent is 4g / L. After the end, the adsorption tail liquid and sulfuric acid are used to prepare the leaching agent, the sulfuric acid concentration is 4g / L, and the heap leaching spray operation is carried out; the leaching agent sprayed every day is 10% of the ore amount, and the leaching stop time ratio is 2:1; when the U concentration of the leaching solution flowing out of the ore heap is <20mg / L, use clean water to wash the heap for 1d, unload the heap, take the tailings, and analyze the uranium content of the tailings. After leaching for 45 days, the uranium leaching rate of the slag is 74.5%, 78.7%, and 81.9%, so the ore particle size is selected to be -3mm.

[0063] Test use A total of 3 columns were used for comparative tests. The ore amount was 5 kg, the spraying amount was 10%, the spraying ratio was 2:1, and the ore particle size was -3 mm. First, it was sprayed with clean water, and then with 10 g / L sulfuric acid solution. When the pH of the leaching solution was <2.0, the leaching agent containing mixed bacteria was sprayed. The spraying time was 8 days, 5 days, and 3 days respectively. The bacterial liquid content in the leaching agent was 15%, and the number of bacteria was about 1×10 7 / ml, the concentration of sulfuric acid in the leaching agent is 4g / L. After the end, the adsorption tail liquid and sulfuric acid are used to prepare the leaching agent, and the sulfuric acid concentration is 4g / L, and the heap leaching spray operation is carried out; the leaching agent sprayed every day is 10% of the ore amount, and the leaching stop time ratio is 2:1; when the U concentration of the leaching solution flowing out of the ore heap is <20mg / L, use clean water to wash the heap for 1d, unload the heap, take the tailings, and analyze the uranium content of the tailings. After leaching for 45 days, the uranium leaching rate of the slag is 81.9%, 81.9%, and 78.7%, so the spraying time of the leaching agent containing mixed bacteria is selected as 5d.

Claims

1. A leaching method for sulfur-containing siliceous mudstone type uranium ore, characterized in that: The steps include: (1) crushing sulfur-containing siliceous mudstone-type uranium ore; (2) piling the sulfur-containing siliceous uranium ore crushed in step (1); (3) wetting the pile built in step (2) with water; (4) acid preleaching the ore using a sulfuric acid solution; (5) After the acid pre-leaching is completed, the ore is sprayed with a leaching agent containing microorganisms to perform microbial leaching; (6) After the microorganisms are leached out, continue to use a solution containing sulfuric acid for spraying acid leaching; (7) Extracting uranium by ion exchange from the leaching solution obtained in steps (4), (5), and (6).

2. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1, characterized in that: The pyrite content of the sulfur-containing siliceous mudstone-type uranium ore in step (1) is greater than 5%.

3. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1 or 2, characterized in that: Step (1) crushing the sulfur-containing siliceous mudstone-type uranium ore to an ore particle size of -5 mm.

4. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1, characterized in that: The concentration of the sulfuric acid solution used in step (4) is 5-10 g / L; the dosage is 5%-30% of the mass of the ore. When the pH of the leaching solution to be discharged is less than 2.0, the spraying of the sulfuric acid solution is stopped.

5. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1 or 4, characterized in that: In step (5), when the pH of the leaching solution flowing out of the ore pile in step (4) is less than 2.0, the adsorption tail liquid containing microorganisms is sprayed as a leaching agent, the sulfuric acid concentration in the leaching agent is 2-5 g / L, and the number of bacteria is not less than 1×10 7 The content of bacterial liquid in the logarithmic growth phase is 5% to 30% per ml; the spraying time is 3 to 7 days; the spraying leaching agent is 10% to 25% of the ore mass, and the daily leaching agent spraying time and stop time are 2:

1.

6. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1, 4 or 5, characterized in that: Microorganisms include: Acidophilic iron-oxidizing bacteria and sulfur-oxidizing bacteria, such as at least two of Thiobacillus ferrooxidans, Thiobacillus thiooxidans, and Microspirillum ferrooxidans; The bacteria were inoculated into the adsorption tail liquid of step (7) at a ratio of 5% to 30% for acclimatization and culture at a temperature of 20 to 35°C and a pH of 1.5 to 2.0 until the bacterial solution concentration reached 1.0×10 7 / mL or more, the redox potential is not less than 470mV, and the culture is acclimated for 3 to 5 times.

7. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1, characterized in that: In step (6), a solution containing sulfuric acid is used as a leaching agent to continue spray leaching the ore pile, and the concentration of sulfuric acid in the leaching agent is 2 to 5 g / L.

8. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1 or 7, characterized in that: In step (6), water or adsorption tail liquid and sulfuric acid are used to prepare a leaching agent.

9. The leaching method of sulfur-containing siliceous mudstone type uranium ore according to claim 1, 7 or 8, characterized in that: Step (6) When the concentration of the leaching solution U flowing out of the ore pile is less than 20 mg / L, water is used for washing and unloading.