Eutectic light casting alloy resistant to high-temperature oxidation at 800DEG C
Through TiAl20.5Si8.5Zr5.0Nb10 eutectic alloy, the problem of easy oxidation at above 800℃ is solved, and better oxidation resistance and mechanical performance stability is achieved. It is suitable for the manufacturing of high-temperature lightweight parts. .
Patent Information
- Application Number
- CN202410987210.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing high-temperature titanium alloys are prone to oxidation at above 800℃, causing the oxide layer to fall off, reducing its resistance to high-temperature oxidation and creep resistance, and it is difficult to meet the high-temperature and corrosion resistance requirements of aviation engine components.
TiAl20.5Si8.5Zr5.0Nb10 eutectic lightweight casting alloy was used to form (Ti, Zr, Nb)3 (Al, Si) and (Ti, Zr, Nb)5 (Si, Al)3 solid solution by regulating the element ratio. The phase and compounds improve the oxidation resistance of the alloy and maintain the stability of the mechanical properties at 800°C.
The alloy exhibits better resistance to high-temperature oxidation at 800°C, the oxide layer has no peeling off, the Nb doping effect reduces the diffusion of O2-, and the density is close to that of the traditional titanium alloy TC4, which is suitable for manufacturing high-temperature, lightweight heat-resistant zero part.
Smart Images

Figure CN118910469A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high temperature resistant structural materials, and is a lightweight casting alloy suitable for working in high temperature (800°C) and oxygen environment. Background Art
[0002] At present, aircraft engines are in service under high temperature, high pressure and high speed conditions, which requires high-temperature alloys to have properties such as high temperature resistance, air flow corrosion resistance and stress corrosion resistance, that is, to achieve a good match between strength, plasticity, toughness, creep resistance and fatigue resistance, and high oxidation resistance at service temperature. At present, the only high-temperature alloys that can fully meet the technical requirements are cobalt-based, iron-based and nickel-based high-temperature alloys, but their specific gravity is large and the fuel utilization rate is not high.
[0003] In order to improve fuel efficiency and engine thrust-to-weight ratio, it is necessary to reduce the weight of its components. At present, high-temperature titanium alloys are not only low in density but also have sufficient high-temperature strength, making them a good candidate. Compared with iron-based and nickel-based high-temperature alloys, lightweight high-temperature titanium alloys have obvious advantages when the operating temperature is lower than 600°C. They have now been included in the sequence of engine materials and have become an important structural material in modern aircraft engines. However, 600°C is the biggest "thermal barrier" encountered in the development of traditional disordered solid solution-strengthened high-temperature titanium alloys. The main reasons are as follows: (1) Above 600°C, the solid solution strengthening and α2 phase and silicide precipitation strengthening effects of the original alloy system have basically reached their limits, and further alloying is difficult to ensure the most basic performance requirements; (2) 600°C is the oxidation resistance limit of traditional high-temperature titanium alloys. Surface oxidation of the alloy reduces thermal stability and fatigue performance, bringing great risks to the application of the material.
[0004] High temperature titanium alloy Ti60 (TiAl 5.6 Sn 4.8 Zr 2.0 Mo 1.0 Si 0.35 Nd 0.8 ) as an example, below 600℃, Ti60 alloy has good comprehensive mechanical properties and high temperature oxidation resistance, because the alloying elements Zr, Si and Nd play a positive role during oxidation, such as Zr promotes oxide nucleation to refine the grains and prevent O atom reaction, Si inhibits Ti 4+ The activity inhibits the formation of TiO2 phase, while Nd can enhance the bonding strength between the oxide layer and the substrate. However, when the operating temperature rises to 800℃
[0005] Its high temperature oxidation resistance and creep resistance deteriorate, and the oxidation weight gain after 100h at 800℃ exceeds 100.0g / m 2, cracks appeared in the oxide layer and gradually expanded, eventually causing the outermost oxide film to fall off, exposing the second oxide film. Further magnification analysis revealed that the Sn- and Nd-rich precipitates caused the surrounding grains to oxidize, and eventually led to the cracking and shedding of the oxide film, such as Figure 1 shown.
[0006] Therefore, how to improve the defect of high-temperature titanium alloy that is easily oxidized during use, improve the corrosion resistance of the alloy and maintain the stability of mechanical properties under high temperature conditions is an issue that the industry urgently needs to solve. Summary of the invention
[0007] A main purpose of the present invention is to overcome at least one defect of the above-mentioned prior art and to provide a eutectic lightweight casting alloy that can improve the shortcoming of high-temperature titanium alloy that is easily oxidized during use, improve the corrosion resistance of the alloy and maintain the stability of mechanical properties under high temperature conditions.
[0008] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:
[0009] According to one aspect of the present invention, a eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius is provided, wherein the nominal composition of the alloy is TiAl 20.5 Si 8.5 Zr 5.0 Nb 10 The atomic percentage of each element is Al: 20.0%-21.0%, Si: 8.0%-9.0%, Zr: 4.5%-5.5%, Nb: 8.0%-10.5%, and the rest is Ti.
[0010] According to one embodiment of the present invention, the density of the alloy is 4.49 g / cm 3 The solidus and liquidus temperatures are 1581.2℃ and 1589.5℃ respectively. The original microstructure at room temperature is short and narrow lamellar, consisting of (Ti,Zr,Nb)3(Al,Si) solid solution phase and (Ti,Zr,Nb)5(Si,Al)3 compound.
[0011] As one embodiment of the present invention, the distribution of each element in the alloy is as follows: the segregation trends of Ti element and Al element are consistent or nearly consistent, while the segregation trends of Si element and Zr element are consistent or nearly consistent, the Nb element is uniformly distributed in each component phase of the alloy, and the distribution of Si is fine and dispersed.
[0012] As an embodiment of the present invention, the alloy composition ratio is Ti: 56.0%, Al: 20.5%, Si: 8.5%, Zr: 5.0%, and Nb: 10.0%.
[0013] As in one embodiment of the present invention, after oxidation at 800°C / 24h, the oxide layer on the surface of the alloy is mainly TiO, the oxide layer does not fall off, and a small amount of Nb in the diffusion layer 5+ Reducing O through doping effect 2- The alloy reaches an oxidation resistant level due to the diffusion of
[0014] It can be seen from the above technical solution that the advantages and positive effects of the eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius of the present invention are:
[0015] In the present invention, the alloy is mainly Ti, and 8.0%-10.5% Nb is used. Its density is similar to that of the traditional titanium alloy TC4, and the crystallization temperature range is small, only 8.3°C. The microstructure is mainly short and narrow lamellar distribution, showing a eutectic structure morphology. The alloy in the present invention not only has the advantages of good fluidity, small segregation and dense structure, but also has better high-temperature oxidation resistance than high-temperature titanium alloy Ti60 without the protection of a protective layer, especially at 800°C. This alloy is very suitable for occasions with high requirements for lightweight, high temperature resistance and oxidation resistance, and can be used to manufacture heat-resistant parts blanks with complex structures and high service temperatures, such as low-pressure compressor blade castings. Thereby improving the disadvantage of high-temperature titanium alloys that they are easy to oxidize during use, improving the corrosion resistance of the alloy and maintaining the stability of mechanical properties under high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The oxidized surface of the high temperature titanium alloy Ti60 in the prior art;
[0017] Figure 2 The TiAl 20.5 Si 8.5 Zr 5.0 Nb 10 OM and SEM structures of the alloy;
[0018] Figure 3 The TiAl 20.5 Si 8.5 Zr 5.0 Nb 10 Element distribution of alloys;
[0019] Figure 4 The kinetic curves of Example 1, Comparative Examples 1 and 4 after oxidation at 600°C / 24h;
[0020] Figure 5 The kinetic curves of Example 2, Comparative Examples 2 and 5 after oxidation at 800°C / 24h;
[0021] Figure 6 The kinetic curves of Example 3, Comparative Examples 3 and 6 after oxidation at 1000°C / 24h;
[0022] Figure 7 The surface structure after oxidation at 600°C / 24h of the present invention;
[0023] Figure 8 The surface structure after oxidation at 800°C / 24h of the present invention;
[0024] Fig. 9 The surface structure after oxidation at 1000°C / 24h of the present invention;
[0025] Fig.10 This is the cross-sectional structure after oxidation at 600°C / 24h of the present invention;
[0026] Fig.11 This is the cross-sectional structure after oxidation at 800°C / 24h of the present invention;
[0027] Fig.12 This is the cross-sectional structure after oxidation at 1000°C / 24h of the present invention;
[0028] Fig.13 This is the XRD spectrum of the oxide layer after 600°C / 24h of the present invention;
[0029] Fig.14 This is the XRD spectrum of the oxide layer after 800°C / 24h of the present invention;
[0030] Fig.15 This is the XRD spectrum of the oxide layer after 000°C / 24h of the present invention. DETAILED DESCRIPTION
[0031] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that the present invention will be comprehensive and complete and fully convey the concepts of the example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their detailed description will be omitted.
[0032] In the following description of different examples of the present invention, reference is made to the accompanying drawings, which form a part of the present invention and in which different exemplary structures, systems and steps that can implement multiple aspects of the present invention are shown by way of example. It should be understood that other specific schemes of components, structures, exemplary devices, systems and steps can be used, and structural and functional modifications can be made without departing from the scope of the present invention. Moreover, although the terms "top", "bottom", "front", "rear", "side", etc. may be used in this specification to describe different exemplary features and elements of the present invention, these terms are used herein only for convenience, such as according to the direction of the examples described in the accompanying drawings. Nothing in this specification should be construed as requiring a specific three-dimensional orientation of the structure to fall within the scope of the present invention.
[0033] According to one aspect of the present invention, a eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius is provided, wherein the nominal composition of the alloy is TiAl 20.5 Si 8.5 Zr 5.0 Nb 10 The atomic percentage of each element is Al: 20.0%-21.0%, Si: 8.0%-9.0%, Zr: 4.5%-5.5%, Nb: 8.0%-10.5%, and the rest is Ti.
[0034] According to one embodiment of the present invention, the density of the alloy is 4.49 g / cm 3 The solidus and liquidus temperatures are 1581.2℃ and 1589.5℃ respectively. The original microstructure at room temperature is short and narrow lamellar, consisting of (Ti,Zr,Nb)3(Al,Si) solid solution phase and (Ti,Zr,Nb)5(Si,Al)3 compound.
[0035] As one embodiment of the present invention, the distribution of each element in the alloy is as follows: the segregation trends of Ti element and Al element are consistent or nearly consistent, while the segregation trends of Si element and Zr element are consistent or nearly consistent, the Nb element is uniformly distributed in each component phase of the alloy, and the distribution of Si is fine and dispersed.
[0036] As an embodiment of the present invention, the alloy composition ratio is Ti: 56.0%, Al: 20.5%, Si: 8.5%, Zr: 5.0%, and Nb: 10.0%.
[0037] As in one embodiment of the present invention, after oxidation at 800°C / 24h, the oxide layer on the surface of the alloy is mainly TiO, the oxide layer does not fall off, and a small amount of Nb in the diffusion layer 5+ Reducing O through doping effect 2- The alloy reaches an oxidation resistant level due to the diffusion of
[0038] It can be seen from the above technical solution that the advantages and positive effects of the eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius of the present invention are:
[0039] In the present invention, the alloy is mainly Ti, and 8.0%-10.5% Nb is used. Its density is similar to that of the traditional titanium alloy TC4, and the crystallization temperature range is small, only 8.3°C. The microstructure is mainly short and narrow lamellar distribution, showing a eutectic structure morphology. The alloy in the present invention not only has the advantages of good fluidity, small segregation and dense structure, but also has better high-temperature oxidation resistance than high-temperature titanium alloy Ti60 without the protection of a protective layer, especially at 800°C. This alloy is very suitable for occasions with high requirements for lightweight, high temperature resistance and oxidation resistance, and can be used to manufacture heat-resistant parts blanks with complex structures and high service temperatures, such as low-pressure compressor blade castings. Thereby improving the disadvantage of high-temperature titanium alloys that they are easy to oxidize during use, improving the corrosion resistance of the alloy and maintaining the stability of mechanical properties under high temperature conditions.
[0040] The alloy of the present invention uses the α2-like phase as the matrix, and forms a eutectic alloy by adjusting the ratio of each element, achieving a good match between high-temperature oxidation resistance and high-temperature mechanical properties. The alloy is very suitable for production using a casting process, especially for the casting production of high-temperature resistant and complex structural parts, and the tensile strength at a high temperature of 600°C is higher than that at room temperature. It has the typical characteristics of an ordered metal-based compound, that is, the strength of the alloy increases with increasing temperature. This abnormal phenomenon is different from the traditional disordered solid solution strengthened high-temperature titanium alloy.
[0041] The density of the alloy of the present invention is equivalent to that of titanium alloy, which is 4.49 g / cm 3 The solidus and liquidus temperatures are 1581.2℃ and 1589.5℃ respectively. The original microstructure at room temperature is short and narrow lamellar, composed of (Ti, Zr, Nb)3(Al, Si) solid solution phase and (Ti, Zr, Nb)5(Si, Al)3 compound. The OM and SEM structures are as follows: Figure 2 shown.
[0042] The distribution of the elements in the alloy of the present invention is as follows: the segregation trends of Ti and Al are basically the same, while the segregation trends of Si and Zr are almost the same, Nb is evenly distributed in each component phase of the alloy, and Si is finely and dispersedly distributed, such as Figure 3 shown.
[0043] The mechanical properties of the alloy of the present invention are shown in Table 1.
[0044]
[0045] The high temperature oxidation resistance of the alloy of the present invention is better than that of high temperature titanium alloy. The main performances are as follows:
[0046] (1) After oxidation at 600℃ / 24h, the oxide film on the alloy surface is mainly TiO. The dense TiO film formed by oxidation adheres to the alloy surface, protecting the alloy matrix from the invasion of O atoms. The oxidation level of the alloy is completely anti-oxidation. (2) After oxidation at 800℃ / 24h, the oxide layer on the alloy surface is still mainly TiO. The oxide layer of the alloy does not fall off. A small amount of Nb in the diffusion layer 5+ Through the doping effect, the O 2- The alloy has a diffusion capacity of 1000℃ / 24h, and the oxidation level of the alloy is oxidation-resistant. (3) After oxidation at 1000℃ / 24h, the oxide layer on the surface of the alloy is mainly TiO2, and discontinuous Nb2O5 is generated at the oxide layer / matrix interface. Internal oxidation occurs in some parts of the alloy, but the oxide layer of the alloy does not fall off. The Nb 5+ The doping effect gradually weakens and the oxidation level of the alloy is sub-anti-oxidation level.
[0047] Mechanism analysis: After the matrix Ti is oxidized, Ti2O, TiO and TiO2 are generated on the alloy surface in sequence. 4+ Excess, stable oxide TiO2 is an N-type semiconductor, and the defect equation is as follows:
[0048]
[0049] That is, when TiO2 is doped with Nb2O5, the concentration of interstitial Ti ions in TiO2 decreases, which also reduces the growth rate of loose TiO2. Therefore, adding Nb can improve the high-temperature oxidation resistance of Ti-based alloys.
[0050] The present invention designs and prepares TiAl 20.5 Si 8.5 Zr 5.0 -Nbx (x = 5, 10 and 15at.%) refractory light alloys, named C2, C3 and C4 alloys respectively. The high temperature oxidation resistance of the three alloys was evaluated by the changes in the microstructure and composition of the samples after constant temperature cyclic oxidation at 600℃, 800℃ and 1000℃. The raw materials used are high purity titanium (99.995wt.%), high purity aluminum (99.99wt.%), high purity silicon (99.99wt.%), high purity zirconium (99.995wt.%) and high purity niobium (99.995wt.%). A vacuum tungsten arc melting furnace was used as the melting equipment to prepare 15g alloy button ingots, and the ingots were processed into strip samples using a diamond cutting machine; high temperature oxidation experiments were carried out in a box-type resistance furnace.
[0051] First, use a vernier caliper to measure the length, width and height of the sample to obtain the surface area of the sample, then place the sample in a cylindrical ceramic crucible that has been pre-burned to a constant weight, use an analytical balance to measure the original weight before oxidation, and record the measured value; second, start the box-type resistance furnace and set the experimental temperature. When the furnace temperature rises to the experimental temperature, place the three alloy samples in the uniform temperature zone of the furnace and keep them warm according to the predetermined oxidation time, which is 2h, 4h, 8h, 15h and 24h respectively; finally, in each time period of the oxidation experiment, all the samples with the crucible need to be taken out, and the crucible cover should be quickly covered to prevent external contamination of the sample or the oxide layer from splashing due to too fast cooling; after air cooling to room temperature, remove the crucible cover, and use an analytical balance to weigh the three groups of samples with crucibles left for each alloy. After the experiment, calculate the average oxidation weight gain and average oxidation rate of the samples under different experimental conditions.
[0052] Example 1
[0053] The specific alloy composition ratio is 56.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 10.0% Nb, and the experimental temperature is 600°C.
[0054] The surface color of the sample after oxidation is light gray, no oxide layer falls off, and the oxidation product is mainly TiO; the oxidation kinetic curve is as follows Figure 4 As shown in Figure 2, the average oxidation rates of the alloys are 0.067 g·m -2 ·h -1 The surface structure of the alloy is arranged in bundles without obvious protrusions. The surface structure still retains traces of diamond wire cutting, and fine oxide phases are evenly distributed on the surface of the alloy. The cross-sectional photos of the oxide layer show that the oxide film is relatively thin and there is almost no diffusion layer, which indicates that the oxide film is formed by the direct reaction of alloy elements and O2. The complete and dense oxide film hinders the migration of O atoms into the matrix.
[0055] Example 2
[0056] The specific alloy composition ratio is 56.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 10.0% Nb, and the experimental temperature is 800°C.
[0057] The surface color of the sample after oxidation is red-gray, no oxide layer falls off, and the oxidation product is mainly TiO; the oxidation kinetic curve is as follows Figure 5 As shown in Figure 2, the average oxidation rates of the alloys are 0.279 g·m -2 ·h -1; Compared with Example 1, the oxide particles of the alloy are obviously coarsened, there are no obvious protrusions on the surface, and the surface structure still retains bundled stripes, indicating that less oxide is generated on the surface and it is difficult to completely cover the processing traces, but the morphology of the second phase is blocky; the cross-sectional photograph of the oxide layer shows that the oxide layer is very thin, the oxide layer is well bonded to the diffusion layer, and no holes or microcracks appear.
[0058] Example 3
[0059] The specific alloy composition ratio is 56.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 10.0% Nb, and the experimental temperature is 1000°C.
[0060] After oxidation, the overall surface color of the sample is light gray, and the alloy surface shows grayish-white patches of varying sizes. The area between the patches is still light gray, and there is no oxide layer falling off. The oxidation product is mainly TiO2. The oxidation kinetic curve is as follows: Figure 6 As shown in Figure 2, the average oxidation rates of the alloys are 1.06 g·m -2 ·h -1 The surface particles of the alloy are small and worm-like, and there are also a small number of large blocky particles. The cross-sectional photograph of the oxide layer shows that the oxidation morphology of the alloy is similar to that of Example 2, with a thicker oxide layer and a thinner and denser diffusion layer.
[0061] Comparative Example 1
[0062] The specific alloy composition ratio is 61.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 5.0% Nb, and the experimental temperature is 600°C.
[0063] The surface color of the sample after oxidation is black-gray, and no oxide layer falls off. The oxidation product is mainly TiO. For the oxidation kinetics curve, see Figure 4 As shown in Figure 2, the average oxidation rates of the alloys are 0.050 g·m -2 ·h -1 The surface structure of the alloy is arranged in bundles without obvious protrusions. The surface structure still retains traces of diamond wire cutting, and fine oxide phases are evenly distributed on the surface of the alloy. The cross-sectional photos of the oxide layer show that the oxide film is relatively thin and there is almost no diffusion layer, which indicates that the oxide film is formed by the direct reaction of alloy elements and O2. The complete and dense oxide film hinders the migration of O atoms into the matrix.
[0064] Comparative Example 2
[0065] The specific alloy composition ratio is 61.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 5.0% Nb, and the experimental temperature is 800°C.
[0066] The surface color of the sample after oxidation is black-gray, which is slightly darker than that of comparative example 1. No oxide layer falls off, and the oxidation product is mainly TiO2. The oxidation kinetic curve is shown in Figure 5 As shown in Figure 2, the average oxidation rates of the alloys are 0.635 g·m -2 ·h -1 The arrangement of oxide particles on the alloy surface becomes disordered, the morphology of the second phase is distributed in clusters, the alloy surface is uneven, the oxide grows rapidly on the alloy surface and obliterates the processing traces; the cross-sectional photograph of the oxide layer shows that a diffusion layer appears at the interface between the alloy oxide layer and the matrix, and the diffusion layer is relatively thick.
[0067] Comparative Example 3
[0068] The specific alloy composition ratio is 61.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 5.0% Nb, and the experimental temperature is 1000°C.
[0069] The surface color of the sample after oxidation is dark gray, no oxide layer falls off, and the oxidation product is mainly TiO2; the oxidation kinetics curve is shown in Figure 6 As shown in Figure 2, the average oxidation rates of the alloys are 1.22 g·m -2 ·h -1 ; The surface of the alloy is composed of larger blocky particles; The cross-sectional photograph of the oxide layer shows that the alloy has no diffusion layer, and the thickness of the oxide layer is equivalent to the total thickness of the oxide layer + diffusion layer in Comparative Example 2.
[0070] Comparative Example 4
[0071] The specific alloy composition ratio is 51.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 15.0% Nb, and the experimental temperature is 600°C.
[0072] The surface color of the sample after oxidation is grayish white, and no oxide layer falls off. The oxidation product is mainly TiO. For the oxidation kinetics curve, see Figure 4 As shown in Figure 2, the average oxidation rates of the alloys are 0.085 g·m -2 ·h -1 The surface structure of the alloy is arranged in bundles without obvious protrusions. The surface structure still retains traces of diamond wire cutting, and fine oxide phases are evenly distributed on the surface of the alloy. The cross-sectional photos of the oxide layer show that the oxide film is relatively thin and there is almost no diffusion layer, which indicates that the oxide film is formed by the direct reaction of alloy elements and O2. The complete and dense oxide film hinders the migration of O atoms into the matrix.
[0073] Comparative Example 5
[0074] The specific alloy composition ratio is 51.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 15.0% Nb, and the experimental temperature is 800°C.
[0075] The surface color of the sample after oxidation is blue-gray, and no oxide layer falls off. The oxidation product is mainly TiO. For the oxidation kinetic curve, see Figure 5 As shown in Figure 2, the average oxidation rates of the alloys are 0.199 g·m -2 ·h -1 ; Compared with Comparative Example 4, the oxide particles of the alloy are obviously coarsened, there are no obvious protrusions on the surface, and the surface structure still retains bundled stripes, indicating that less oxide is generated on the surface and it is difficult to completely cover the processing traces, but the morphology of the second phase is blocky; the cross-sectional photograph of the oxide layer shows that a diffusion layer appears at the interface between the alloy oxide layer and the substrate. The thickness of the diffusion layer is much thicker than that of Example 2, but thinner than that of the diffusion layer of Comparative Example 2.
[0076] Comparative Example 6
[0077] The specific alloy composition ratio is 51.0% Ti, 20.5% Al, 8.5% Si, 5.0% Zr, 15.0% Nb, and the experimental temperature is 1000°C.
[0078] The oxidized surface color of the sample after oxidation is grayish white as a whole, with unevenly dispersed dark loose block areas on the surface. The oxidation product is mainly TiO2; the oxidation kinetic curve is shown in Figure 6 As shown in the figure, the average oxidation rates of the alloys are 1.12 g·m -2 ·h -1 ; The surface of the alloy is almost entirely composed of fine particles, and large holes appear on the surface. These holes will merge over time, seriously damaging the protective effect of the oxide film, thereby deteriorating the antioxidant performance; the cross-sectional photograph of the oxide layer shows that the oxide layer and the diffusion layer of the alloy are obviously thicker than those in Example 5, and there are multiple long and thin linear displays at the interface between the oxide layer and the diffusion layer. These microcracks can easily cause the oxide layer to crack or even fall off.
[0079] Figure 7 The surface structure after oxidation at 600°C / 24h of the present invention;
[0080] Figure 8 This is the surface structure after oxidation at 800°C / 24h of the present invention;
[0081] Fig. 9 The surface structure after oxidation at 1000°C / 24h of the present invention;
[0082] Fig.10 This is the cross-sectional structure after oxidation at 600°C / 24h of the present invention;
[0083] Fig.11 This is the cross-sectional structure after oxidation at 800°C / 24h of the present invention;
[0084] Fig.12 This is the cross-sectional structure after oxidation at 1000°C / 24h of the present invention;
[0085] Fig.13 This is the XRD spectrum of the oxide layer after 600°C / 24h of the present invention;
[0086] Fig.14 This is the XRD spectrum of the oxide layer after 800°C / 24h of the present invention;
[0087] Fig.15 This is the XRD spectrum of the oxide layer after 000°C / 24h of the present invention.
[0088] In the present invention, the surface structure and cross-sectional structure of the samples were oxidized at 600°C / 24h, 800°C / 24h and 1000°C / 24h. Figure 7-12 As shown, the XRD patterns of different oxide layers are also shown Figure 13-15 shown.
[0089] Those skilled in the art should understand that the specific structures and processes shown in the above specific embodiments are only exemplary and not restrictive. Moreover, those skilled in the art can combine the various technical features shown above in various possible ways to form new technical solutions, or make other changes, which are all within the scope of the present invention.
Claims
1. A eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius, characterized in that: The nominal composition of the alloy is TiAl 20.5 Si 8.5 Zr 5.0 Nb 10 The atomic percentage of each element is Al: 20.0%-21.0%, Si: 8.0%-9.0%, Zr: 4.5%-5.5%, Nb: 8.0%-10.5%, and the rest is Ti.
2. The eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius according to claim 1, characterized in that: The density of the alloy is 4.49 g / cm 3 The solidus and liquidus temperatures are 1581.2℃ and 1589.5℃ respectively. The original microstructure at room temperature is short and narrow lamellar, consisting of (Ti,Zr,Nb)3(Al,Si) solid solution phase and (Ti,Zr,Nb)5(Si,Al)3 compound.
3. The eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius according to claim 2, characterized in that: The distribution of each element in the alloy is as follows: the segregation trends of Ti and Al are consistent or nearly consistent, while the segregation trends of Si and Zr are consistent or nearly consistent, the Nb element is evenly distributed in each component phase of the alloy, and the distribution of Si is fine and dispersed.
4. The eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius according to any one of claims 1 to 3, characterized in that: The alloy composition ratio is Ti: 56.0%, Al: 20.5%, Si: 8.5%, Zr: 5.0%, and Nb: 10.0%.
5. The eutectic lightweight casting alloy resistant to high temperature oxidation at 800 degrees Celsius according to claim 4, characterized in that: After oxidation at 800℃ / 24h, the oxide layer on the surface of the alloy is mainly TiO, the oxide layer does not fall off, and a small amount of Nb in the diffusion layer 5+ Reducing O through doping effect 2- The alloy reaches an oxidation resistant level due to the diffusion of