Efficient corrosion-resistant aluminum-copper alloy grounding material and preparation method thereof
By adding rare earth metal and zinc to the grounding material to form a protective film and achieving the combination of copper and carbon in heat treatment, the problem of corrosionability of the grounding material in a wet soil environment is solved, and the corrosion resistance and stability of the material are significantly improved. suitable for power systems.
Patent Information
- Application Number
- CN202410911405.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
AI Technical Summary
Grounding materials are prone to corrosion in wet soil environments, resulting in insufficient corrosion resistance, affecting the stability and safety of the power system.
Using high-efficiency corrosion-resistant aluminum-copper alloy materials, the copper oxide and aluminum oxide protective film is formed by adding rare earth metals, magnesium and zinc to the carbon composite porous copper, and the in-situ redox reaction of copper and carbon is realized in heat treatment, combined with Rare earth elements refine grains and purify grain boundaries to improve the corrosion resistance of the material.
It significantly improves the corrosion resistance of grounding materials, reduces stress corrosion, enhances the stability and safety of materials, and is suitable for long-term and reliable power system applications.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of grounding materials, and in particular to a high-efficiency corrosion-resistant aluminum-copper alloy grounding material and a preparation method thereof. Background Art
[0002] Grounding materials play a vital role in the grounding system of power transmission lines. The grounding system is an indispensable part of the power system. It can connect equipment, buildings, etc. to the earth to ensure the safety of equipment and personnel. In important places such as power plants and substations, long-term, reliable and stable grounding systems are required to ensure the safety of equipment and personnel. Therefore, during design and construction, it is necessary to fully consider the selection of grounding materials and connection methods to ensure the quality and stability of the grounding system.
[0003] However, grounding materials are often in a moist soil environment, which is prone to corrosion. Therefore, it is necessary to solve the corrosion resistance problem of grounding materials. Summary of the invention
[0004] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a high-efficiency corrosion-resistant aluminum-copper alloy grounding material and a preparation method thereof.
[0005] The technical solution of the present invention is as follows:
[0006] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, characterized by comprising the following raw materials in parts by weight:
[0007] 10-20 parts of carbon composite porous copper, 50-70 parts of aluminum, 0.1-0.5 parts of rare earth metals, 0.1-0.3 parts of magnesium, 1-3 parts of zinc;
[0008] The preparation method of the carbon composite porous copper is as follows:
[0009] The wood fiber is pretreated, then immersed in a copper salt solution, a hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0010] As a preferred embodiment of the present invention, the pretreatment is specifically: subjecting the wood fiber to plasma treatment, then sequentially adding it to ice water and 30-50° C. hydrogel, and finally freeze-drying it.
[0011] As a preferred embodiment of the present invention, the plasma treatment conditions are: in an air atmosphere, the treatment voltage is 5-15V, and the treatment time is 5-10min.
[0012] As a preferred embodiment of the present invention, the treatment is carried out in ice water for 5-10 minutes, and in the hydrogel for 10-20 minutes.
[0013] As a preferred embodiment of the present invention, the preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, heated at 40-50° C., and sodium bisulfite is added after cooling.
[0014] As a preferred embodiment of the present invention, the heat treatment temperature is 1800-2200°C.
[0015] As a preferred embodiment of the present invention, the rare earth element is at least one of lanthanum, cerium, neodymium and yttrium.
[0016] The present invention also discloses a method for preparing any of the above high-efficiency corrosion-resistant aluminum-copper alloy grounding materials, which comprises taking raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0017] As a preferred embodiment of the present invention, the melting temperature is 800-1000°C, and the casting temperature is 700-800°C.
[0018] The beneficial effects of the present invention are:
[0019] (1) The invention discloses a highly efficient and corrosion-resistant aluminum-copper alloy grounding material. By adding a composite carbon porous copper material, copper is mixed in the pores of the carbon material. Then, cuprous oxide is formed on the surface of the copper in a dry air atmosphere. During the subsequent heat treatment, cuprous oxide and carbon with a graphite structure undergo an in-situ redox reaction, thereby achieving a firm combination of copper and carbon atoms. This is more conducive to the subsequent molten casting with other metals, greatly improving the high corrosion resistance of the grounding material.
[0020] (2) The addition of aluminum and zinc elements to the highly efficient and corrosion-resistant aluminum-copper alloy grounding material of the present invention can form an aluminum oxide protective film on the alloy surface, thereby improving the corrosion resistance. The addition of an appropriate amount of magnesium can reduce stress corrosion; in addition, the addition of a small amount of rare earth elements can not only facilitate alloy preparation, but also effectively refine the grains, purify the grain boundaries, and further improve the corrosion resistance of the material. DETAILED DESCRIPTION
[0021] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0022] Example 1
[0023] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0024] 10 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0025] The preparation method of the carbon composite porous copper is as follows:
[0026] The wood fiber is pretreated, then immersed in a 4 mol / L cupric chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0027] The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 40° C. hydrogel, and finally freeze-drying the wood fiber.
[0028] The plasma treatment conditions are: in air atmosphere, treatment voltage 10V, treatment time 8min.
[0029] Treat in ice water for 8 min and in hydrogel for 15 min.
[0030] The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, and then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, and the mixture is heated at 40-50° C., and sodium bisulfite is added after cooling, wherein the mass ratio of the sodium alginate, polyvinyl alcohol, sodium dodecylbenzene sulfonate, octadecyl methacrylate and sodium sulfite is 5:15:1:1:1:0.2.
[0031] The heat treatment temperature is 2000°C.
[0032] The rare earth element is lanthanum.
[0033] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0034] The melting temperature is 950°C, and the casting temperature is 750°C.
[0035] Example 2
[0036] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0037] 15 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0038] The preparation method of the carbon composite porous copper is as follows:
[0039] The wood fiber is pretreated, then immersed in a 4 mol / L cupric chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0040] The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 40° C. hydrogel, and finally freeze-drying the wood fiber.
[0041] The plasma treatment conditions are: in air atmosphere, treatment voltage 10V, treatment time 8min.
[0042] Treat in ice water for 8 min and in hydrogel for 15 min.
[0043] The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, and then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, and the mixture is heated at 40-50° C., and sodium bisulfite is added after cooling, wherein the mass ratio of the sodium alginate, polyvinyl alcohol, sodium dodecylbenzene sulfonate, octadecyl methacrylate and sodium sulfite is 5:15:1:1:1:0.2.
[0044] The heat treatment temperature is 2000°C.
[0045] The rare earth element is lanthanum.
[0046] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0047] The melting temperature is 950°C, and the casting temperature is 750°C.
[0048] Example 3
[0049] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0050] 20 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0051] The preparation method of the carbon composite porous copper is as follows:
[0052] The wood fiber is pretreated, then immersed in a 4 mol / L cupric chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0053] The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 40° C. hydrogel, and finally freeze-drying the wood fiber.
[0054] The plasma treatment conditions are: in air atmosphere, treatment voltage 10V, treatment time 8min.
[0055] Treat in ice water for 8 min and in hydrogel for 15 min.
[0056] The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, and then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, and the mixture is heated at 40-50° C., and sodium bisulfite is added after cooling, wherein the mass ratio of the sodium alginate, polyvinyl alcohol, sodium dodecylbenzene sulfonate, octadecyl methacrylate and sodium sulfite is 5:15:1:1:1:0.2.
[0057] The heat treatment temperature is 2000°C.
[0058] The rare earth element is lanthanum.
[0059] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0060] The melting temperature is 950°C, and the casting temperature is 750°C.
[0061] Example 4
[0062] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0063] 15 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0064] The preparation method of the carbon composite porous copper is as follows:
[0065] The wood fiber is pretreated, then immersed in a 4 mol / L cupric chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0066] The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 40° C. hydrogel, and finally freeze-drying the wood fiber.
[0067] The plasma treatment conditions are: in air atmosphere, treatment voltage 15V, treatment time 5min.
[0068] Treat in ice water for 8 min and in hydrogel for 15 min.
[0069] The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, and then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, and the mixture is heated at 40-50° C., and sodium bisulfite is added after cooling, wherein the mass ratio of the sodium alginate, polyvinyl alcohol, sodium dodecylbenzene sulfonate, octadecyl methacrylate and sodium sulfite is 5:15:1:1:1:0.2.
[0070] The heat treatment temperature is 2000°C.
[0071] The rare earth element is cerium.
[0072] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0073] The melting temperature is 950°C, and the casting temperature is 750°C.
[0074] Example 5
[0075] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0076] 15 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0077] The preparation method of the carbon composite porous copper is as follows:
[0078] The wood fiber is pretreated, then immersed in a 4 mol / L cupric chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0079] The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 40° C. hydrogel, and finally freeze-drying the wood fiber.
[0080] The plasma treatment conditions are: in air atmosphere, treatment voltage 15V, treatment time 5min.
[0081] Treat in ice water for 9 min and in hydrogel for 20 min.
[0082] The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, and then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, and the mixture is heated at 40-50° C., and sodium bisulfite is added after cooling, wherein the mass ratio of the sodium alginate, polyvinyl alcohol, sodium dodecylbenzene sulfonate, octadecyl methacrylate and sodium sulfite is 5:15:1:1:1:0.2.
[0083] The heat treatment temperature is 2000°C.
[0084] The rare earth element is yttrium.
[0085] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0086] The melting temperature is 950°C, and the casting temperature is 750°C.
[0087] Comparative Example 1 (without pretreatment)
[0088] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0089] 20 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0090] The preparation method of the carbon composite porous copper is as follows:
[0091] The wood fiber is immersed in a 4 mol / L copper chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
[0092] The heat treatment temperature is 2000°C.
[0093] The rare earth element is lanthanum.
[0094] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0095] The melting temperature is 950°C, and the casting temperature is 750°C.
[0096] Comparative Example 2 (No Surface Oxidation)
[0097] A high-efficiency, corrosion-resistant aluminum-copper alloy grounding material, comprising the following raw materials in parts by weight:
[0098] 20 parts of carbon composite porous copper, 60 parts of aluminum, 0.3 parts of rare earth metals, 0.3 parts of magnesium, 2 parts of zinc;
[0099] The preparation method of the carbon composite porous copper is as follows:
[0100] The wood fiber is pretreated, then immersed in a 4 mol / L copper chloride solution, 20 mL of a 35 wt% hydrazine hydrate solution is added dropwise, the precipitate is dried, and then heat-treated in a reducing atmosphere to obtain the product.
[0101] The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 40° C. hydrogel, and finally freeze-drying the wood fiber.
[0102] The plasma treatment conditions are: in air atmosphere, treatment voltage 10V, treatment time 8min.
[0103] Treat in ice water for 8 min and in hydrogel for 15 min.
[0104] The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, and then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, and the mixture is heated at 40-50° C., and sodium bisulfite is added after cooling, wherein the mass ratio of the sodium alginate, polyvinyl alcohol, sodium dodecylbenzene sulfonate, octadecyl methacrylate and sodium sulfite is 5:15:1:1:1:0.2.
[0105] The heat treatment temperature is 2000°C.
[0106] The rare earth element is lanthanum.
[0107] A method for preparing a highly efficient corrosion-resistant aluminum-copper alloy grounding material comprises taking the above raw materials, mixing and melting them, and then refining, casting and processing them in sequence to obtain the grounding material.
[0108] The melting temperature is 950°C, and the casting temperature is 750°C.
[0109] The above embodiments and comparative examples were subjected to performance tests, and the test results are shown in Table 1.
[0110] Corrosion effect test: According to GB / T16545-1996 "Removal of corrosion products on corrosion specimens of metals and alloys", mechanical and chemical methods are used to remove corrosion products on the specimens, and then the specimens are dried and weighed, and the corrosion weight loss is calculated.
[0111] Table 1 Performance test results of embodiments and comparative examples
[0112] Sample Weight loss (g) Average corrosion depth (μm) Resistivity(Ω.m) Example 1 0.0054 2.01 <![CDATA[1.62×10 -2 ]]> Example 2 0.0051 1.92 <![CDATA[1.58×10 -2 <!-- 5 -->]]> Example 3 0.0053 1.95 <![CDATA[1.61×10 -2 ]]> Example 4 0.0057 2.05 <![CDATA[1.65×10 -2 ]]> Example 5 0.0055 2.03 <![CDATA[1.64×10 -2 ]]> Comparative Example 1 0.0125 2.51 <![CDATA[1.97×10 -2 ]]> Comparative Example 2 0.0091 2.46 <![CDATA[1.82×10 -2 ]]>
[0113] It can be seen from the above table that the performance of the grounding material of the embodiment is better than that of the comparative example. The main reasons may be as follows: by adding the composite carbon porous copper material, the copper element is intercalated in the pores of the carbon material, and then in a dry air atmosphere, cuprous oxide is formed on the surface of the copper element. During the subsequent heat treatment, the cuprous oxide and the carbon with a graphite structure undergo an in-situ redox reaction, thereby achieving a firm bond between copper and carbon atoms. This is more conducive to greatly improving the high corrosion resistance of the grounding material during subsequent molten casting with other metals. In addition, the addition of aluminum and zinc elements can form an aluminum oxide protective film on the surface of the alloy, thereby improving the corrosion resistance. The addition of an appropriate amount of magnesium can reduce stress corrosion; in addition, the addition of a small amount of rare earth elements can not only facilitate alloy preparation, but also effectively refine the grains, purify the grain boundaries, and further improve the corrosion resistance of the material.
[0114] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention.
Claims
1. A highly efficient and corrosion-resistant aluminum-copper alloy grounding material, characterized in that: The invention comprises the following raw materials in parts by weight: 10-20 parts of carbon composite porous copper, 50-70 parts of aluminum, 0.1-0.5 parts of rare earth metals, 0.1-0.3 parts of magnesium, 1-3 parts of zinc; The preparation method of the carbon composite porous copper is as follows: The wood fiber is pretreated, then immersed in a copper salt solution, a hydrazine hydrate solution is added dropwise, the precipitate is dried, and then placed in dry air so that the surface of the copper element is oxidized with cuprous oxide, and then heat-treated in a reducing atmosphere to obtain the product.
2. The high-efficiency, corrosion-resistant aluminum-copper alloy grounding material according to claim 1 is characterized in that: The pretreatment specifically includes: subjecting the wood fiber to plasma treatment, then sequentially adding the wood fiber to ice water and 30-50° C. hydrogel, and finally freeze-drying the wood fiber.
3. The high-efficiency, corrosion-resistant aluminum-copper alloy grounding material according to claim 2 is characterized in that: The plasma treatment conditions are: in an air atmosphere, a treatment voltage of 5-15V, and a treatment time of 5-10min.
4. The high-efficiency, corrosion-resistant aluminum-copper alloy grounding material according to claim 2 is characterized in that: Treat in ice water for 5-10 min and in hydrogel for 10-20 min.
5. The high-efficiency corrosion-resistant aluminum-copper alloy grounding material according to claim 2 is characterized in that: The preparation method of the hydrogel is as follows: sodium alginate and polyvinyl alcohol are mixed and heated, then sodium dodecylbenzene sulfonate and octadecyl methacrylate are added, heated at 40-50° C., and sodium bisulfite is added after cooling.
6. The high-efficiency, corrosion-resistant aluminum-copper alloy grounding material according to claim 1 is characterized in that: The heat treatment temperature is 1800-2200°C.
7. The high-efficiency, corrosion-resistant aluminum-copper alloy grounding material according to claim 1 is characterized in that: The rare earth element is at least one of lanthanum, cerium, neodymium and yttrium.
8. A method for preparing a high-efficiency corrosion-resistant aluminum-copper alloy grounding material according to any one of claims 1 to 7, characterized in that: The raw materials are taken, mixed and melted, and then refined, cast and processed in sequence to obtain the grounding material.
9. The method for preparing a high-efficiency corrosion-resistant aluminum-copper alloy grounding material according to claim 8, characterized in that: The melting temperature is 800-1000°C, and the casting temperature is 700-800°C.