Material for realizing MnNiGe-based alloy violent magnetic field driven variable magnetic phase change, and preparation method and application thereof

The magnetization strength of the MnNiGe-based alloy is adjusted through Fe element substitution and secondary annealing, and the magnetic field-driven variable magnetic martensite phase transformation is achieved, solving the problem of difficult driving of the magnetic field in the MnNiGe-based alloy, and is suitable for a variety of magnetic function applications.

CN118910487APending Publication Date: 2024-11-08国瑞科创稀土功能材料(赣州)有限公司 +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410990981.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The second type of magnetic martensite phase transformation in MnNiGe-based alloy can only be induced by temperature, and the magnetic field is difficult to drive, limiting the application of room temperature magnetic refrigeration technology.

Method used

By replacing the Mn element with Fe element and performing secondary annealing, the magnetization strength of the MnNiGe-based alloy and the sensitivity of the martensite phase transition to the magnetic field are adjusted, and the variable magnetic martensite phase transition driven by the magnetic field is realized.

Benefits of technology

Under temperature or pressure conditions, the material undergoes a phase change between the strong magnetic martensite phase and the weak magnetic austenite phase, and a variable magnetic martensite phase change is realized under magnetic field drive, increasing the driving force of the phase change , suitable for thermal magnetoelectric conversion, magnetostriction, magnetic drive and solid state refrigeration devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910487A_ABST
    Figure CN118910487A_ABST
Patent Text Reader

Abstract

The invention provides a material for achieving MnNiGe-based alloy violent magnetic field driven variable magnetic phase change and a preparation method and application of the material. The chemical formula of the material is Mn < 1-x > FexNiGe. Wherein x is greater than or equal to 0 and less than or equal to 0.50, and x represents atomic percentage content. According to the preparation method of the material, the magnetization intensity of the MnNiGe-based alloy and the sensitive degree of martensite phase transformation to a magnetic field are adjusted by replacing the Mn element with the Fe element in the MnNiGe-based alloy and conducting secondary annealing, and magnetic field-driven variable-magnetism martensite phase transformation is achieved while temperature-driven martensite phase transformation occurs. Therefore, the material is subjected to martensite phase transformation between a strong magnetic martensite phase and a weak magnetic austenite phase under the temperature or pressure (internal pressure or external pressure), magnetic field driven variable magnetic martensite phase transformation can also be achieved, and the obtained MnNiGe-based alloy has the advantages of being easy to machine into a thin strip, high in mechanical strength and the like. The material can be used in the fields of thermomagnetoelectric conversion, magnetostriction, magnetic / heat sensitive elements, magnetic driving, solid-state refrigeration devices and the like due to the characteristics of strong magnetism and temperature (magnetic field) driven variable magnetism martensite phase transformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnetic phase change, and in particular to a material for realizing a violent magnetic field driven magnetic phase change of a MnNiGe-based alloy, and a preparation method and application thereof. Background Art

[0002] Near-magnetic refrigeration technology is based on the country's major needs for energy conservation, emission reduction, low carbon and high efficiency. It also caters to the key supporting technology for cutting-edge research such as providing extreme physical environments and improving instrument resolution. Magnetic refrigeration technology based on magnetocaloric effect has more significant advantages in refrigeration efficiency and environmental protection than traditional gas compression refrigeration. Magnetic refrigeration technology near room temperature is particularly important in the fields of intelligent manufacturing, national defense and military industry, and people's livelihood projects.

[0003] The magnetization intensity of the primary phase change alloy changes dramatically near the phase change point, accompanied by a large magnetocaloric effect, and exhibits a variety of physical effects. External stimuli such as light, force, electricity, heat, and magnetism may cause changes in the system energy, thereby inducing phase change. 2 In-type structured MnNiGe-based alloys can undergo magnetic structural phase transitions near room temperature, accompanied by unique giant magnetocaloric, magnetoresistance, magneto-induced strain, and magnetic shape memory effects. The phase transition of MnNiGe-based alloys is adjustable, with two types of primary magnetic structural phase transitions. The first type is to controllably increase the martensitic transformation temperature T t ~197℃ down to parent phase Ni 2 Curie transition temperature T of In type structure C A ~-68℃ and the Nel transformation temperature T of the martensitic phase TiNiSi type structure N M The temperature range between 73℃ and 83℃ is used to establish the magneto-structural coupling phase transition. The first type of magneto-structural coupling phase transition is controlled by T below room temperature. C A , which limits the application of room temperature magnetic refrigeration technology. The second type is to flip the antiferromagnetism of the martensite phase into ferromagnetism and adjust the martensite transformation temperature T t Reduced to parent phase Ni 2 Curie transition temperature of In type structure and Curie transition temperature of martensitic TiNiSi type structure T C M The temperature range between 200 and 200 °C makes the magnetic-structural coupling phase transition occur in a wide temperature range near room temperature. Through the second type of phase transition regulation, the difference in magnetization intensity near the phase transition of this type of material becomes larger, and the temperature range of phase transition is widened, which is expected to be used in room temperature magnetic refrigeration.

[0004] For MnNiGe-based alloys, the second type of magnetic martensitic phase transition can almost only be induced by temperature and is difficult to be driven by a magnetic field. Therefore, achieving a drastic magnetic field-driven magnetic phase transition in MnNiGe-based alloys is the direction of scientific research and technical work. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a material for realizing a magnetically variable phase transition driven by a severe magnetic field in a MnNiGe-based alloy, and a preparation method and application thereof. The material for driving a magnetically variable phase transition not only causes the material to undergo a martensitic phase transition between a strong magnetic martensite phase and a weak magnetic austenite phase under temperature or pressure (internal pressure or external pressure), but can also drive a magnetically variable martensitic phase transition. The obtained MnNiGe-based alloy can be used in the fields of thermomagnetic-electric conversion, magnetostriction, magnetic drive, solid-state refrigeration devices, etc.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The first object of the present invention is to provide a material for realizing a magnetic phase change driven by a severe magnetic field in a MnNiGe-based alloy. The chemical formula of the magnetic phase change material driven by a severe magnetic field in a MnNiGe-based alloy is Mn 1-x Fe x NiGe; wherein 0≤x≤0.50, x represents the atomic percentage content.

[0008] The second object of the present invention is to provide a method for preparing a material that realizes a severe magnetic field-driven variable magnetic phase transition of a MnNiGe-based alloy, wherein the magnetization intensity of the MnNiGe-based alloy and the sensitivity of the martensitic phase transition to the magnetic field are adjusted by replacing the Mn element with the Fe element and performing secondary annealing, and a magnetic field-driven variable magnetic martensitic phase transition is realized while a temperature-driven martensitic phase transition occurs.

[0009] Preferably, the method for preparing the material for realizing the severe magnetic field driven variable magnetic phase transition of the MnNiGe-based alloy comprises the following steps:

[0010] Calculate the required mass of Mn, Ni, Fe, Ge elements according to the stoichiometric ratio and prepare the ingredients;

[0011] Arc melting was used to obtain alloy ingot samples;

[0012] The alloy ingot sample was placed in a quartz tube with an inner diameter of 10 mm and one end was closed. The vacuum degree in the quartz tube was evacuated to below 3 Pa, and 0.5 atmospheres of argon gas was filled in for purging. This process was repeated 4 times. After the last purging, the vacuum degree was evacuated to below 3 Pa again.

[0013] The elongated quartz tube is then quickly burned off with an acetylene flame, so that the alloy ingot sample is sealed in a vacuum quartz tube. The sealed quartz tube is placed in a high-temperature furnace for heat treatment to obtain a bulk sample.

[0014] Preferably, the method for preparing the material for realizing the severe magnetic field driven variable magnetic phase transition of the MnNiGe-based alloy comprises the following steps:

[0015] Calculate the required mass of Mn, Ni, Fe, Ge elements according to the stoichiometric ratio and prepare the ingredients;

[0016] Arc melting was used to obtain alloy ingot samples;

[0017] The melt rapid quenching method was used to make the above alloy ingot samples into rapid quenching strip samples;

[0018] The above-mentioned rapidly quenched strip sample was placed in a quartz tube with an inner diameter of 10 mm and one end was closed. The vacuum degree in the quartz tube was evacuated to below 3 Pa, and 0.5 atmospheres of argon gas was filled in for gas washing. This process was repeated 4 times. After the last gas washing, the vacuum degree was evacuated to below 3 Pa again.

[0019] Then, the elongated quartz tube is quickly burned off with an acetylene flame, so that the strip sample is sealed in a vacuum quartz tube. The sealed quartz tube is placed in a high-temperature furnace for heat treatment to obtain the strip sample.

[0020] Preferably, the heat treatment is quenching, followed by secondary annealing; wherein the quenching temperature is 600-850°C, and the quenching treatment time is 96-168h; the secondary annealing temperature is 300-1200°C, and the secondary annealing treatment time is 0-120h.

[0021] Preferably, the mass of the prepared Mn, Ni, Fe, and Ge elemental single substances needs to be accurate to two decimal places in milligram units, and the purity of the single substances needs to be controlled at more than 99.95%.

[0022] Preferably, during the arc melting, the raw materials are placed in a water-cooled copper crucible arc furnace, and the vacuum degree of the melting furnace is drawn to 5×10 -3 Pa, fill with argon gas with a purity of 99.999% at 0.8 atmospheres for arc melting;

[0023] For the first smelting, use 27A current to melt the metal. When the molten metal in the crucible flows, turn the block sample from the first smelting over, increase the current to 40A and smelt it 4 more times to obtain the alloy ingot.

[0024] Preferably, during the melt rapid quenching, a portion of the alloy ingot samples obtained by smelting is placed in a quartz tube with a bottom hole diameter of 6 to 10 mm, the quartz tube is installed in an induction coil of a high vacuum melt rapid quenching device, the distance between the quartz tube and the copper roller is adjusted up and down by about 2 mm, the vacuum degree of the device is evacuated to below 8×10-4Pa, and argon gas with a purity of 99.999% at 0.8 atmospheres is filled to perform melt rapid quenching;

[0025] The copper roller speed is adjusted to the required speed, which is 10 to 40 m / s. After the copper roller speed is stable, the heating power supply current is adjusted, and the ingot is melted through the high-frequency induction coil until it covers the lower end of the quartz tube. The air pressure difference is used to push the molten metal liquid through the bottom of the quartz tube and spray onto the copper roller with a stable speed to obtain a fast-quenching strip sample at a specific strip throwing speed.

[0026] The third object of the present invention is to provide a material that realizes a violent magnetic field driven magnetic phase change of a MnNiGe-based alloy and its application in thermomagnetic electric conversion, magnetostriction, magnetic drive, magnetic / thermal sensitive elements and solid-state refrigeration devices.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. Mn provided by the present invention 1-x Fe x In addition to the properties of common magnetic phase change materials, such as temperature or pressure (internal pressure or external pressure) can cause the material to undergo a martensitic phase transition between a strong magnetic martensite phase and a weak magnetic austenite phase, the NiGe-based alloy also has the characteristic of a magnetic field-driven variable magnetic martensitic phase transition. This is because the phase transition can be induced by temperature or driven by a magnetic field. The reason is that the magnetization intensities of the martensite and austenite phases before and after the phase transition are different. Through secondary annealing, the difference in magnetization intensity before and after the phase transition increases, and the Zeeman energy generated by applying an external magnetic field increases, thereby increasing the driving force for the phase transition.

[0029] 2. Mn provided by the present invention 1-x Fe x NiGe alloy has the characteristics of easy processing into thin strips, strong magnetism and temperature (magnetic field) driven variable magnetic martensitic phase transformation.

[0030] 3. Mn provided by the present invention 1-x Fe x NiGe alloys have multifunctional properties near the phase transition, including giant magnetocaloric effect, negative thermal expansion, magneto-induced strain, etc., and can be widely used in solid-state refrigeration devices, magnetic drives, magnetic / thermal sensitive elements, thermo-magnetoelectric conversion and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The room temperature XRD patterns of the alloys provided in Examples 1-4 of the present invention;

[0032] Figure 2 The isofield thermomagnetic curves of the alloys provided in Examples 1-4 of the present invention;

[0033] Figure 3 The differential scanning calorimetry curves of the alloys provided in Examples 1-4 of the present invention;

[0034] Figure 4 The isofield thermomagnetic curves of the alloys provided in Examples 5-7 of the present invention;

[0035] Figure 5 Isothermal magnetization curves of the alloys provided in Examples 5-7 of the present invention, wherein Figure (a) is the isothermal magnetization curve of the rapidly quenched sample; Figure (b) is the isothermal magnetization curve of the sample after secondary annealing at a temperature of 500°C for 10 h; Figure (c) is the isothermal magnetization curve of the sample after secondary annealing at a temperature of 700°C for 10 h; Figure (d) is the isothermal magnetization curve of the sample after secondary annealing at a temperature of 900°C for 10 h. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Since the steps and methods used are the same as those in Examples 1-7, in order to avoid redundancy, the present invention describes a preferred embodiment, but the present invention is not limited thereto, but can also be specifically implemented in other ways within the scope of the technical solution defined in the attached claims.

[0038] According to the composition Mn 1-x Fe x NiGe and other materials are used to make corresponding bulk samples or strip samples, and obtain the ideal first-order magnetic structure phase transition and its corresponding magneto-induced effects (magnetocaloric effect, magnetoresistance effect, magneto-induced strain)

[0039] The present invention adjusts the magnetization intensity of the alloy and the sensitivity of the martensitic phase transformation to the magnetic field by replacing the Mn element with the Fe element in the alloy and performing secondary annealing, and realizes the magnetic field-driven variable magnetic martensitic phase transformation while the temperature-driven martensitic phase transformation occurs.

[0040] Based on the above principle, the actual alloy chemical formula is Mn 1-x Fe xNiGe; wherein 0≤x≤0.50, x represents the atomic percentage content.

[0041] The technical solution of the present invention is further illustrated below in the form of specific examples.

[0042] Example 1

[0043] To satisfy the alloy's chemical formula Mn 1-x Fe x NiGe, x is 0.16. This embodiment 1 is an alloy Mn with variable magnetic martensitic phase transformation 0.84 Fe 0.16 NiGe.

[0044] The method for preparing a material for realizing a severe magnetic field driven variable magnetic phase transition of a MnNiGe-based alloy comprises the following steps:

[0045] The required mass of Mn, Fe, Ni and Ge elements is calculated according to the stoichiometric ratio and the ingredients are prepared with an accuracy of 0.1mg to 0.01mg. The purity of the metal elements is above 99.95%.

[0046] The prepared raw materials are placed in a water-cooled copper crucible arc melting furnace and the vacuum degree is drawn to 5×10 -3 Pa, fill with 0.8 atmospheres of argon gas with a purity of 99.999% for arc melting.

[0047] In the first smelting, use 27A current to melt the metal. When you see the metal liquid flowing in the crucible, turn the block sample over, increase the current slightly to 40A and smelt it 4 more times to get Mn. 0.84 Fe 0.16 NiGe alloy ingot.

[0048] Place some alloy ingot samples in a quartz tube with one end closed. The inner diameter of the quartz tube is 10 mm. Then, the vacuum degree in the quartz tube is evacuated to below 3 Pa and filled with 0.5 atmospheres of argon for gas washing. This is repeated 4 times. After the last gas washing, the vacuum degree is evacuated to below 3 Pa. Then, the stretched quartz tube is quickly burned off with an acetylene flame and the sample is sealed in the vacuum quartz tube.

[0049] The sealed samples were then placed in a high-temperature furnace for annealing heat treatment at a quenching temperature of 850°C for 120 hours. The samples were then taken out and quickly quenched in cold water. The quenched samples were placed in the same high-temperature furnace for secondary annealing at 800°C for 1 hour. The samples were cooled in the furnace to obtain bulk samples with good phase formation and uniformity, and temperature-induced magnetic-structural coupling phase transition was obtained.

[0050] Example 2

[0051] To satisfy the alloy's chemical formula Mn 1-x Fe x NiGe, x is 0.16. This embodiment 2 is an alloy Mn with variable magnetic martensitic phase transformation 0.84 Fe 0.16 NiGe.

[0052] The preparation methods of the material for realizing the severe magnetic field driven magnetic phase transition of the MnNiGe-based alloy in this embodiment 2 and embodiment 1 are almost the same, except that Mn 0.84 Fe 0.16 Heat treatment of NiGe alloy ingot.

[0053] When the sealed sample is placed in a high-temperature furnace for annealing heat treatment, the quenching temperature is 850°C and the quenching time is 120 hours. Then it is taken out and quickly quenched in cold water. The quenched sample is placed in the same high-temperature furnace and annealed again at 800°C for 3 hours. After cooling in the furnace, a bulk sample with good phase formation and uniformity is obtained, and a temperature-induced magnetic-structural coupling phase transition is obtained.

[0054] Example 3

[0055] To satisfy the alloy's chemical formula Mn 1-x Fe x NiGe, x is 0.16. This embodiment 3 is an alloy Mn with variable magnetic martensitic phase transformation 0.84 Fe 0.16 NiGe.

[0056] The preparation method of the material for realizing the severe magnetic field driven magnetic phase transition of the MnNiGe-based alloy in this embodiment 3 is almost the same as that in embodiment 1, except that Mn 0.84 Fe 0.16 Heat treatment of NiGe alloy ingot.

[0057] When the sealed sample is placed in a high-temperature furnace for annealing heat treatment, the quenching temperature is 850°C and the quenching time is 120 hours. Then it is taken out and quickly quenched in cold water. The quenched sample is placed in the same high-temperature furnace and annealed again at 800°C for 6 hours. After cooling in the furnace, a bulk sample with good phase formation and uniformity is obtained, and a temperature-induced magnetic-structural coupling phase transition is obtained.

[0058] Example 4

[0059] To satisfy the alloy's chemical formula Mn 1-x Fe x NiGe, x is 0.16. This embodiment 4 is an alloy Mn with variable magnetic martensitic phase transformation 0.84 Fe 0.16NiGe.

[0060] The preparation methods of the material for realizing the severe magnetic field driven magnetic phase transition of the MnNiGe-based alloy in this embodiment 4 and embodiment 1 are almost the same, except that Mn 0.84 Fe 0.16 Heat treatment of NiGe alloy ingot.

[0061] When the sealed sample is placed in a high-temperature furnace for annealing heat treatment, the quenching temperature is 850°C and the quenching time is 120 hours. Then it is taken out and quickly quenched in cold water. The annealed sample is placed in the same high-temperature furnace and annealed again at 800°C for 10 hours. After cooling in the furnace, a bulk sample with good phase formation and uniformity is obtained, and a temperature-induced magnetic-structural coupling phase transition is obtained.

[0062] Experimental analysis

[0063] The bulk samples prepared in Examples 1-4 were subjected to XRD, isofield thermomagnetic and differential scanning calorimetry analysis respectively.

[0064] (I) XRD analysis

[0065] The room temperature XRD patterns of the bulk samples prepared in Examples 1-4 are shown in the attached figure. Figure 1 As shown by Figure 1 It can be seen that the bulk samples prepared in Examples 1-4 are high-temperature hexagonal Ni 2 In phase, and no second phase exists.

[0066] (II) Analysis of isofield thermal magnetic curves

[0067] The isofield thermomagnetic curves of the bulk samples prepared in Examples 1-4 are shown in the attached figure. Figure 2 As shown by Figure 2 It can be seen that there is an obvious hysteresis in the temperature increase and decrease, and a temperature-induced primary magnetic-structural coupling phase transition from ferromagnetic martensite to paramagnetic austenite occurs.

[0068] (III) Differential scanning calorimetry curve analysis

[0069] The differential scanning calorimetry curves of the bulk samples prepared in Examples 1-4 are shown in the attached figure. Figure 3 As shown by Figure 3 It can be seen that the phase transition temperature is Figure 2 The phase transition temperature of the given equifield thermomagnetic curve corresponds to that of the given equifield thermomagnetic curve.

[0070] Example 5

[0071] To satisfy the alloy's chemical formula Mn 1-x Fe xNiGe, x is 0.16. This embodiment 6 is an alloy Mn with variable magnetic martensitic phase transformation 0.84 Fe 0.16 NiGe.

[0072] The preparation method of the material for realizing the severe magnetic field driven magnetic phase transition of the MnNiGe-based alloy in this embodiment 5 is almost the same as that in embodiment 1, except that Mn 0.84 Fe 0.16 Heat treatment of NiGe alloy ingot.

[0073] When the sealed sample is placed in a high-temperature furnace for annealing heat treatment, the quenching temperature is 850°C and the quenching time is 120 hours. Then it is taken out and quickly quenched in cold water. The quenched sample is placed in the same high-temperature furnace and annealed for the second time at 500°C for 10 hours. It is cooled in the furnace to obtain a block sample with good phase formation and uniformity.

[0074] Example 6 satisfies the chemical formula of the alloy Mn 1-x Fe x NiGe, x is 0.16. This embodiment 6 is an alloy Mn with variable magnetic martensitic phase transformation 0.84 Fe 0.16 NiGe.

[0075] The preparation method of the material for realizing the severe magnetic field driven magnetic phase transition of the MnNiGe-based alloy in this embodiment 6 is almost the same as that in embodiment 1, except that Mn 0.84 Fe 0.16 Heat treatment of NiGe alloy ingot.

[0076] When the sealed sample is placed in a high-temperature furnace for annealing heat treatment, the quenching temperature is 850°C and the quenching time is 120 hours. Then it is taken out and quickly quenched in cold water. The quenched sample is placed in the same high-temperature furnace and annealed again at 700°C for 10 hours. After cooling in the furnace, a block sample with good phase formation and uniformity is obtained.

[0077] Example 7

[0078] The preparation methods of the material for realizing the severe magnetic field driven magnetic phase transition of the MnNiGe-based alloy in this embodiment 7 are almost the same as those in embodiment 1, except that Mn 0.84 Fe 0.16 Heat treatment of NiGe alloy ingot.

[0079] When the sealed sample is placed in a high-temperature furnace for annealing heat treatment, the quenching temperature is 850°C and the quenching time is 120 hours. Then it is taken out and quickly quenched in cold water. The quenched sample is placed in the same high-temperature furnace and annealed for the second time at 900°C for 10 hours. After cooling in the furnace, a block sample with good phase formation and uniformity is obtained.

[0080] Experimental analysis

[0081] The bulk samples prepared in Examples 5-7 are subjected to isofield thermal magnetic and isothermal magnetization curves respectively.

[0082] (I) Analysis of isofield thermal magnetic curves

[0083] The block samples prepared in Examples 5-7 were subjected to isofield thermomagnetic curve testing. The results of the isofield thermomagnetic curve testing are shown in the attached figure. Figure 4 As shown, Figure 4 It shows that as the temperature decreases, a magnetic martensite phase transformation occurs from weak magnetic austenite to strong magnetic martensite, and the magnetization intensity of the alloy increases significantly.

[0084] (II) Analysis of isothermal magnetization curves

[0085] The isothermal magnetization curves of the bulk samples prepared in Examples 5-7 are shown in the attached figure. Figure 5 The measurement of isothermal magnetization curve adopts the "cycle method", that is, before each temperature measurement, the temperature must be raised by zero field to make the sample enter a weak magnetic state, and then the zero field is lowered to the measurement temperature to measure the magnetization curve. Figure 5 It can be seen that a violent magnetic field-driven variable magnetism martensitic phase transformation is obtained in this composition. At lower temperatures, the alloy magnetization increases slowly with the increase of the magnetic field, and there is still no saturation trend at a magnetic field of up to 7T, indicating that the alloy is in a weak magnetic state at low temperatures; at higher temperatures, the alloy magnetization increases rapidly with the increase of the magnetic field and gradually tends to saturation, indicating that the alloy is in a ferromagnetic state at higher temperatures.

[0086] At 255K, the alloy has an obvious magnetic field-driven metamagnetic phase transition, in which the H req ~1.7T, H comp ~5.2T, the difference in magnetization intensity is as high as 42.53Am2kg -1 ; H of the sample prepared in Example 6 req ~2.0T, H comp ~4.9T, the difference in magnetization intensity is 29.92Am2kg -1 ; H of the sample prepared in Example 7 req ~1.6T, H comp ~5.3T, the difference in magnetization intensity is 38.75Am2kg -1This suggests that a variety of magnetic functional properties can be achieved in alloys of this composition.

[0087] Then, according to the isothermal magnetization curve, the ΔSM and RC values ​​of the samples prepared in Examples 5-7 under 0-5T and 0-7T magnetic field changes were calculated using Maxwell's formula, and the results are shown in Table 1. For example, the isothermal magnetic entropy change ΔS of the sample prepared in Example 5 under 0-5T magnetic field M ~29.3Jkg -1 K -1 Refrigeration capacity RC~217.4Jkg -1 Such a large magnetic entropy change is attributed to the drastic magnetic-driven phase transition of the sample, which results in an ideal first-order magnetic structure phase transition and its magnetocaloric effect.

[0088] Table 1 shows the ΔSM and RC values ​​of the alloys provided in Examples 5-7 of the present invention under 0-5T and 0-7T magnetic fields.

[0089]

[0090]

[0091] Any of the methods for realizing severe magnetic field driven variable magnetic phase transition of MnNiGe based alloys in Examples 1 to 7 has the property of causing the material to undergo a martensitic phase transition between a strong magnetic martensite phase and a weak magnetic austenite phase under the above-mentioned conditions of temperature, magnetic field or pressure (internal pressure or external pressure). It can be inferred that the above-mentioned method for preparing severe magnetic field driven variable magnetic phase transition of MnNiGe based alloys can realize a magnetic field driven variable magnetic phase transition while a temperature driven martensitic phase transition occurs when the value is taken as the two endpoints of the numerical range and any value between the two endpoints.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A material for realizing a magnetic phase transition of a MnNiGe-based alloy driven by a severe magnetic field, characterized in that: The chemical formula of the MnNiGe-based alloy violent magnetic field driven magnetic phase change material is Mn 1-x Fe x NiGe; wherein 0≤x≤0.50, x represents the atomic percentage content.

2. A method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 1, characterized in that: In the MnNiGe-based alloy, the magnetization intensity of the MnNiGe-based alloy and the sensitivity of the martensitic phase transformation to the magnetic field are adjusted by replacing the Mn element with the Fe element and performing secondary annealing, and a magnetic field-driven variable magnetism martensitic phase transformation is achieved while a temperature-driven martensitic phase transformation occurs.

3. The method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 2, characterized in that: The steps include: Calculate the required mass of Mn, Ni, Fe, Ge elements according to the stoichiometric ratio and prepare the ingredients; Arc melting was used to obtain alloy ingot samples; The alloy ingot sample was placed in a quartz tube with an inner diameter of 10 mm and one end was closed. The vacuum degree in the quartz tube was evacuated to below 3 Pa, and 0.5 atmospheres of argon gas was filled in for purging. This process was repeated 4 times. After the last purging, the vacuum degree was evacuated to below 3 Pa again. The elongated quartz tube is then quickly burned off with an acetylene flame, so that the alloy ingot sample is sealed in a vacuum quartz tube. The sealed quartz tube is placed in a high-temperature furnace for heat treatment to obtain a bulk sample.

4. The method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 2, characterized in that: The steps include: Calculate the required mass of Mn, Ni, Fe, Ge elements according to the stoichiometric ratio and prepare the ingredients; Arc melting was used to obtain alloy ingot samples; The melt rapid quenching method was used to make the above alloy ingot samples into rapid quenching strip samples; The above-mentioned rapidly quenched strip sample was placed in a quartz tube with an inner diameter of 10 mm and one end was closed. The vacuum degree in the quartz tube was evacuated to below 3 Pa, and 0.5 atmospheres of argon gas was filled in for gas washing. This process was repeated 4 times. After the last gas washing, the vacuum degree was evacuated to below 3 Pa again. Then, the elongated quartz tube is quickly burned off with an acetylene flame, so that the strip sample is sealed in a vacuum quartz tube. The sealed quartz tube is placed in a high-temperature furnace for heat treatment to obtain the strip sample.

5. A method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 3 or 4, characterized in that: The heat treatment is quenching, followed by secondary annealing; wherein the quenching temperature is 600-850°C, and the quenching treatment time is 96-168h; the secondary annealing temperature is 300-1200°C, and the secondary annealing treatment time is 0-120h.

6. A method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 3 or 4, characterized in that: The mass of the prepared Mn, Ni, Fe, and Ge elements must be accurate to two decimal places in milligrams, and the purity of the elements must be controlled above 99.95%.

7. A method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 3 or 4, characterized in that: During the arc melting, the raw materials are placed in a water-cooled copper crucible arc furnace, and the vacuum degree of the melting furnace is drawn to 5×10 -3 Pa, fill with argon gas with a purity of 99.999% at 0.8 atmospheres for arc melting; For the first smelting, use 27A current to melt the metal. When the molten metal in the crucible flows, turn the block sample from the first smelting over, increase the current to 40A and smelt it 4 more times to obtain the alloy ingot.

8. The method for preparing a material for realizing a severe magnetic field driven magnetic phase transition of a MnNiGe-based alloy as claimed in claim 4, characterized in that: During the melt quenching, a portion of the alloy ingot samples obtained by smelting was placed in a quartz tube with a bottom hole diameter of 6 to 10 mm. The quartz tube was installed in the induction coil of the high vacuum melt quenching equipment. The distance between the quartz tube and the copper roller was adjusted up and down by about 2 mm. The vacuum degree of the equipment was drawn to 8×10 -4 Pa, fill with 0.8 atmospheres of argon gas with a purity of 99.999% to perform rapid quenching of the melt; The copper roller speed is adjusted to the required speed, which is 10 to 40 m / s. After the copper roller speed is stable, the heating power supply current is adjusted, and the ingot is melted through the high-frequency induction coil until it covers the lower end of the quartz tube. The air pressure difference is used to push the molten metal liquid through the bottom of the quartz tube and spray onto the copper roller with a stable speed to obtain a fast-quenching strip sample at a specific strip throwing speed.

9. Application of the material for realizing the severe magnetic field driven magnetic phase transition of MnNiGe based alloy as claimed in claim 1 in thermomagnetic electric conversion, magnetostriction, magnetic drive, magnetic / thermal sensitive elements and solid-state refrigeration devices.

Citation Information

Patent Citations

  • Anisotropic negative thermal expansion material as well as preparation method and application thereof

    CN115216676A