Ni-containing nodular cast iron material as well as preparation method and application thereof
By preparing Ni-containing ductile iron material, and then performing rapid cooling inoculation and spheroidization treatment followed by annealing and tempering, a tempered martensite + retained austenite + graphite spheroid structure is formed, which solves the problem of insufficient wear resistance and toughness of connecting fittings, extends service life and improves corrosion resistance.
Patent Information
- Application Number
- CN202410985323.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
Existing connecting hardware materials have a short service life in the West-to-East Power Transmission Project due to their poor resistance to atmospheric corrosion, poor ductility and toughness, and insufficient wear resistance, which affects the safe and stable operation of the power transmission channels.
Ni-containing ductile iron material is used. After rapid cooling inoculation and spheroidization treatment, it undergoes homogenization annealing and tempering treatment to form a microstructure of tempered martensite + retained austenite + graphite spheroids, which improves the strength, toughness and wear resistance of the material.
It significantly extends the service life of connecting hardware, reduces operation and maintenance costs, improves the corrosion resistance and low friction of materials, and solves the problem of insufficient wear resistance and toughness of existing materials.
Smart Images

Figure CN118910497A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of alloy preparation, and in particular relates to a Ni-containing ductile iron material and a preparation method and application thereof. Background Art
[0002] The eastern region of my country is densely populated, with relatively developed industry and commerce, and a large demand for energy; while the vast majority of fossil energy and clean energy are distributed in the central and western regions of my country, where the population is sparse and the energy demand is relatively small, and the energy deposits and load centers are inversely distributed. With the rapid development of the economy and society, this problem has become increasingly serious. In order to optimize resource allocation, the construction of cross-regional energy regulation channels has become an inevitable choice to promote the high-quality development of my country's economy and society. Therefore, the "West-to-East Power Transmission" project represented by large-capacity and long-distance power transmission methods such as ultra-high voltage transmission has come into being. In the power transmission channel of the West-to-East Power Transmission Project, overhead transmission lines are the main mode of power transmission. However, due to the vast area and complex climate environment in Northwest my country, overhead transmission lines often pass through multiple strong wind / strong sandstorm and acid rain environment areas, resulting in increasingly serious wear and corrosion problems of transmission line connection fittings, causing wear, corrosion, stress fracture and other failures of the connection fittings. Especially in an environment where corrosion and wear act together, friction damage occurs at the contact part of the connection fittings, allowing the corrosive medium to invade and accelerate the failure process. The deformation and failure caused by the deterioration of the performance of the connection hardware may lead to the disconnection of the overhead transmission line, the breaking of the strands, the loss of the insulator string and other faults, which seriously affect the safe and stable operation of the power transmission channel. Therefore, it is of great practical significance to study and improve the wear and corrosion resistance of the connection hardware for the safe operation of the overhead transmission line.
[0003] Ductile iron contains abundant spherical graphite. During the friction and wear process of ductile iron, the graphite in the matrix acts as a solid lubricant to form a low-friction lubricating film, which effectively slows down the wear. At the same time, due to the barrier of graphite balls, the corrosion of ductile iron by the atmospheric environment is suppressed. Therefore, the service life of the connection fittings made of ductile iron is likely to be significantly extended. However, the strength and toughness of ductile iron are very poor, and the appropriate additive elements must be carefully selected to improve ductile iron by alloying. Summary of the invention
[0004] Aiming at the problems existing in the prior art of connection fitting materials such as poor atmospheric corrosion resistance, poor plasticity and toughness, insufficient wear resistance and short service life, the present invention provides a Ni-containing ductile iron material.
[0005] The invention also provides a method for preparing the Ni-containing ductile iron material.
[0006] Another object of the present invention is to provide the use of the above-mentioned Ni-containing ductile iron material in the preparation of connecting hardware manufacturing parts.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The present invention provides a Ni-containing ductile iron material, which comprises the following components by mass percentage:
[0009] 2.51% to 2.53% C, 2.0% to 2.6% Si, 0.14% to 0.15% Mn, 1.4% to 8.1% Ni, ≤0.1% P and ≤0.02% S, with the balance being Fe and unavoidable impurities.
[0010] Preferably, the Ni content is 1.43% to 8.07%.
[0011] The present invention also provides a method for preparing the Ni-containing ductile iron material, comprising the following steps:
[0012] S1: Rapidly cooling the molten iron containing Ni element after inoculation and spheroidization to the pseudo-eutectic region to obtain Ni-containing ductile iron or profiles;
[0013] S2: homogenizing annealing the Ni-containing ductile iron or profile;
[0014] S3: The ductile iron casting or profile after homogenization treatment is heated again and then tempered to obtain Ni-containing ductile iron material.
[0015] Furthermore, in S1, the rapid cooling rate is ≥50°C / s.
[0016] Furthermore, in S2, the annealing method is: heating the ductile iron profile to 950-1050°C, keeping the temperature for 8-12 hours, and then taking it out of the furnace and air-cooling it to room temperature.
[0017] Furthermore, in S3, the reheating treatment is to heat the Ni-containing ductile iron casting or profile to 950°C, keep it at this temperature for 3 hours, and water quench it; the tempering treatment is to heat the Ni-containing ductile iron casting or profile to 500°C, keep it at this temperature for 2 hours, and air cool it.
[0018] Furthermore, the metal matrix structure of the ductile iron material is tempered martensite + retained austenite, and the material structure is tempered martensite + retained austenite + graphite nodules.
[0019] Furthermore, the density of the graphite balls is greater than 500 / mm 2 The ball diameter ranges from 25 to 40 μm, and the ball-ink spacing is 50 μm.
[0020] The present invention also provides the use of the Ni-containing ductile iron material in preparing connection hardware manufacturing parts.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention provides a method for preparing Ni-containing ductile iron material, which comprises the following steps: horizontally continuously casting a completely eutectic profile from Ni-containing molten iron after spheroidization treatment, and then subjecting the obtained profile to homogenization annealing treatment to obtain a Ni-containing ductile iron profile with a high ductile density, and then subjecting the profile to 950°C austenitization for 180 minutes, water quenching, and 500°C tempering for 120 minutes to obtain a structure of tempered martensite, which does not affect the condensation of graphite balls, and has both strengthening and toughening effects, so that the ductile iron has excellent plasticity and toughness, and can reduce the concentration of Fe atoms in the material while causing lattice distortion. At the same time, since the plasticity and toughness of the tempered martensite + residual austenite structure are good, and graphite gives the material good wear resistance and corrosion resistance, the material has the advantages of excellent low friction, corrosion resistance, high strength and toughness, etc., which can effectively improve the problems of the current connection hardware being not resistant to atmospheric corrosion, poor plasticity and toughness, insufficient wear resistance, and low life, and extend the service life of the connection hardware.
[0023] (2) The element composition provided by the present invention can promote the condensation of graphite nodules while improving the strength and toughness of the material, thereby achieving the effect of strengthening and toughening ductile iron.
[0024] (3) The Ni-containing ductile iron material provided by the present invention can reduce the concentration of Fe atoms at the contact interface and cause lattice distortion during corrosion reaction, thereby inhibiting the penetration growth of corrosion products and hindering the slip of dislocations, so that wear cracks cannot extend along the crystal. At the same time, graphite gives the material good corrosion resistance, thereby improving the wear resistance, corrosion resistance and plasticity of ductile iron.
[0025] (3) The present invention also provides a ductile iron manufactured part comprising the above-mentioned Ni-containing ductile iron material, which has the advantages of excellent low friction, corrosion resistance and high strength and toughness, and can effectively improve the current problems of connection fittings being not resistant to atmospheric corrosion and having poor plasticity and toughness, thereby extending the service life of the connection fittings and reducing the operation and maintenance costs of transmission lines. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic flow chart of a method for preparing a Ni-containing ductile iron material according to the present invention;
[0027] Figure 2 A metallographic structure diagram of a Ni-containing ductile iron material without corrosion after rapid cooling to a pseudo-eutectic region and solidification during the preparation process of the material;
[0028] Figure 3 This is a metallographic structure diagram of the ductile iron material with a Ni content of 1.43% prepared in Example 1 of the present invention after rapid cooling to the pseudo-eutectic region and solidification and corrosion;
[0029] Figure 4 This is a metallographic structure diagram of the ductile iron material with a Ni content of 3.43% prepared in Example 2 of the present invention after being rapidly cooled to the pseudo-eutectic region and solidified and then corroded;
[0030] Figure 5 This is a metallographic structure diagram of the ductile iron material with a Ni content of 6.29% prepared in Example 3 of the present invention after rapid cooling to the pseudo-eutectic region and solidification and corrosion;
[0031] Figure 6 This is a metallographic structure diagram of the ductile iron material with a Ni content of 8.07% prepared in Example 4 of the present invention after rapid cooling to the pseudo-eutectic region and solidification and corrosion;
[0032] Figure 7 This is a corroded metallographic structure diagram after water quenching and tempering in the preparation process of a Ni-containing ductile iron material of the present invention. The metallographic structures of the component materials selected in this article after water quenching and tempering are the same;
[0033] Figure 8 This is a graph showing the mass loss of a ductile iron material with a Ni content of 1.43% to 8.07% before and after a corrosion test;
[0034] Fig. 9 The diagram is a surface crack length diagram of a ductile iron material with a Ni content of 1.43% to 8.07% after 800 fatigue tests. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0036] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0037] See also Figure 1 The present invention provides a method for preparing a Ni-containing ductile iron material, comprising the following steps:
[0038] S1: The molten iron after spheroidization is quickly cooled to the pseudo-eutectic zone to obtain a casting or profile with a complete eutectic structure, specifically: the primary iron is melted into molten iron at 1500°C to 1550°C, and the molten iron is inoculated and spheroidized, preferably: the inoculant is 75SiFe, and the amount of the inoculant added is adjustable between 0.20% and 0.60% by mass according to the Si content of the primary iron; the spheroidizing agent is ferrosilicon rare earth magnesium alloy, and the spheroidizing treatment is performed. The molten iron is rapidly cooled to the pseudo-eutectic zone at a rate of ≥50°C / s to complete the solidification of the molten iron, thereby obtaining a casting or profile with a complete eutectic structure; wherein the casting or profile comprises the following components by mass percentage: 2.51% to 2.53% C, 2.0% to 2.6% Si, 0.14% to 0.15% Mn, 1.4% to 8.1% Ni, ≤0.1% P and ≤0.02% S, and the balance is Fe and unavoidable impurities.
[0039] S2: homogenizing the Ni-containing ductile iron profile to fully precipitate the ductile iron and fully dissolve the Ni element into the metal matrix. Specifically:
[0040] The casting or profile is heated to 950-1050°C at a heating rate of 300-500°C / h, kept at this temperature for 8-12h, then taken out of the furnace and air-cooled to room temperature to complete the homogenization treatment.
[0041] S3: The ductile iron casting or profile after homogenization is subjected to water quenching + tempering treatment to obtain a ductile iron material for connecting hardware with a structure of tempered martensite + residual austenite + graphite nodules, specifically:
[0042] The casting or profile after homogenization treatment is heated to 950°C again at a heating rate of 300°C / h, kept at this temperature for 3 hours, then taken out of the furnace and water quenched. Then, the casting or profile is heated to 500°C at a heating rate of 300°C / h, kept at this temperature for 2 hours, and then air-cooled.
[0043] Example 1
[0044] (1) melting primary iron into molten iron at 1500° C. to 1550° C., feeding an inoculant (75SiFe) and a spheroidizing agent (ferrosilicon-rare earth-magnesium alloy) into the molten iron synchronously through a wire feeding system, subjecting the molten iron to inoculation and spheroidizing treatment, rapidly cooling the spheroidized molten iron to a pseudo-eutectic region at a rate of 50° C. / s to complete solidification of the molten iron, and obtaining a casting or profile with a complete eutectic structure; wherein the casting or profile comprises the following components by mass percentage: 2.53% C, 2.56% Si, 0.14% Mn, 1.43% Ni, ≤0.1% P and ≤0.02% S, with the remainder being Fe and unavoidable impurities.
[0045] (2) The casting or profile is heated to 950°C at a heating rate of 300°C / h, kept at this temperature for 12 hours, then removed from the furnace and air-cooled to room temperature to complete the homogenization treatment. The casting or profile after homogenization treatment is heated to 950°C again at a heating rate of 300°C / h, kept at this temperature for 3 hours, then removed from the furnace and water quenched, and then the casting or profile is heated to 500°C at a heating rate of 300°C / h, kept at this temperature for 2 hours, and then air-cooled.
[0046] Example 2
[0047] (1) melting primary iron into molten iron at 1500° C. to 1550° C., feeding an inoculant (75SiFe) and a spheroidizing agent (silicon-iron-rare earth-magnesium alloy) into the molten iron synchronously through a wire feeding system, subjecting the molten iron to inoculation and spheroidizing treatment, rapidly cooling the spheroidized molten iron to a pseudo-eutectic region at a rate of 55° C. / s to complete solidification of the molten iron, and obtaining a casting or profile with a complete eutectic structure; wherein the casting or profile comprises the following components by mass percentage: 2.52% C, 2.22% Si, 0.15% Mn, 3.43% Ni, ≤0.1% P and ≤0.02% S, with the remainder being Fe and unavoidable impurities.
[0048] (2) The casting or profile is heated to 950°C at a heating rate of 300°C / h, kept at this temperature for 12 hours, then removed from the furnace and air-cooled to room temperature to complete the homogenization treatment. The casting or profile after homogenization treatment is heated to 950°C again at a heating rate of 300°C / h, kept at this temperature for 3 hours, then removed from the furnace and water quenched, and then the casting or profile is heated to 500°C at a heating rate of 300°C / h, kept at this temperature for 2 hours, and then air-cooled.
[0049] Example 3
[0050] (1) melting primary iron into molten iron at 1500° C. to 1550° C., feeding an inoculant (75SiFe) and a spheroidizing agent (ferrosilicon-rare earth-magnesium alloy) into the molten iron synchronously through a wire feeding system, subjecting the molten iron to inoculation and spheroidizing treatment, rapidly cooling the spheroidized molten iron to a pseudo-eutectic region at a rate of 55° C. / s to complete solidification of the molten iron, and obtaining a casting or profile with a complete eutectic structure; wherein the casting or profile comprises the following components by mass percentage: 2.52% C, 2.10% Si, 0.15% Mn, 6.29% Ni, ≤0.1% P and ≤0.02% S, with the remainder being Fe and unavoidable impurities.
[0051] (2) The casting or profile is heated to 950°C at a heating rate of 300°C / h, kept at this temperature for 12 hours, then removed from the furnace and air-cooled to room temperature to complete the homogenization treatment. The casting or profile after homogenization treatment is heated to 950°C again at a heating rate of 300°C / h, kept at this temperature for 3 hours, then removed from the furnace and water quenched, and then the casting or profile is heated to 500°C at a heating rate of 300°C / h, kept at this temperature for 2 hours, and then air-cooled.
[0052] Example 4
[0053] (1) Primary iron is melted into molten iron at 1500° C. to 1550° C., an inoculant (75SiFe) and a spheroidizing agent (silicon-iron-rare earth-magnesium alloy) are simultaneously fed into the molten iron using a wire feeding system, the molten iron is inoculated and spheroidized, and the spheroidized molten iron is rapidly cooled to a pseudo-eutectic region at a rate of 55° C. / s to complete solidification of the molten iron, thereby obtaining a casting or profile with a complete eutectic structure; wherein the casting or profile comprises the following components by mass percentage: 2.53% C, 2.05% Si, 0.15% Mn, 8.07% Ni, ≤0.1% P and ≤0.02% S, with the remainder being Fe and unavoidable impurities.
[0054] (2) The casting or profile is heated to 950°C at a heating rate of 300°C / h, kept at this temperature for 12 hours, then removed from the furnace and air-cooled to room temperature to complete the homogenization treatment. The casting or profile after homogenization treatment is heated to 950°C again at a heating rate of 300°C / h, kept at this temperature for 3 hours, then removed from the furnace and water quenched, and then the casting or profile is heated to 500°C at a heating rate of 300°C / h, kept at this temperature for 2 hours, and then air-cooled.
[0055] Effect Example
[0056] The castings or profiles prepared in the process of preparing Ni-containing ductile iron materials in the embodiment were subjected to metallographic microstructure tests, such as Figure 2-7 As shown, the density of spheroidal graphite is 500±30 / mm 2 ; From the figure, it can be seen that the size of the spheroidal graphite in the four samples is relatively uniform, with a ball diameter range of 25-40μm and a spheroidal graphite spacing of 50μm. The metallographic structure of the material before homogenization is different. When the Ni content is 1.4% to 3.4%, it is ferrite + pearlite, when the Ni content is about 6%, it is martensite + residual austenite, and when the Ni content is about 8%, it is martensite + bainite + residual austenite, because the Ni element can stabilize pearlite, expand the austenite phase area, and obtain martensite at room temperature. The structure after quenching + tempering treatment is tempered martensite + residual austenite.
[0057] Figure 8 The following is a comparison of the corrosion weight loss data of Ni-containing ductile iron and H13 die steel after the same time experiment. Figure 7 It can be seen that the corrosion resistance of H13 mold steel is poor, and the corrosion weight loss rate reaches 12.43%; after adding Ni element, the corrosion resistance of Ni-containing ductile iron is significantly improved, and the higher the Ni content, the stronger the corrosion resistance; for example, in Example 4, the corrosion weight loss rate of Ni-containing ductile iron is only 5.2%, which is significantly lower than that of H13 steel.
[0058] Fig. 9The thermal fatigue crack growth results of Ni-containing ductile iron are shown in Figure 2. The thermal fatigue test conditions are to heat the sample to 600°C and keep it at this temperature for 5 minutes, then quickly cool it to room temperature with water. This is a thermal fatigue test cycle. Repeat the above thermal fatigue test and measure the crack length to obtain the crack length results as shown in Figure 2. Figure 8 As shown. As can be seen from the figure, after 800 repeated thermal fatigue tests, the crack length of Ni-containing ductile iron is only micrometer-level; and as the Ni content increases, the thermal fatigue crack length decreases. For example, in the sample of Example 4 with a Ni content of 8.07%, the crack length after 800 thermal fatigue tests is only 52μm. In contrast, the ductile iron reported in the literature ([1] Chen Dan, Wu Suzhen, Wu Lingxian, et al. Effect of thermal fatigue upper limit temperature on thermal fatigue resistance of ductile iron; [2] Lv Dong. Study on thermal fatigue behavior of a heat-resistant ductile iron) has a thermal fatigue crack length much higher than that of the Ni-containing ductile iron proposed in the present invention under milder experimental conditions (heating to 600°C and keeping warm for 3 minutes, then quickly cooling to room temperature with water) and fewer thermal fatigue times. This proves that the addition of Ni element proposed in the present invention in combination with appropriate heat treatment process can significantly improve the toughness of ductile iron.
[0059] In summary, the present invention provides a Ni-containing ductile iron material, a preparation method and a Ni-containing ductile iron manufacturing part, through which the Ni-containing molten iron after spheroidization is horizontally continuously cast into a completely eutectic profile, and then the obtained profile is subjected to homogenization annealing treatment to obtain a Ni-containing ductile iron profile with a high ductile density, and then a 950°C austenitization 180min water quenching + 500°C tempering 120min treatment is performed to obtain a ductile iron profile with a final structure of tempered martensite + residual austenite + graphite balls. The ductile iron provided by the present invention, the combination of various elements, will not affect the condensation of graphite balls, and has a strengthening and toughening effect, and graphite gives the material good atmospheric corrosion resistance, so that the ductile iron has excellent mechanical properties, and thus has the advantages of high atmospheric corrosion resistance, excellent wear resistance and good plastic toughness, etc., which solves the problems that the current connection hardware is not resistant to atmospheric corrosion, has poor plastic toughness, insufficient wear resistance and low life, and prolongs the service life of the connection hardware.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.
Claims
1. A Ni-containing ductile iron material, characterized in that: The invention comprises the following components by mass percentage: 2.51% to 2.53% C, 2.0% to 2.6% Si, 0.14% to 0.15% Mn, 1.4% to 8.1% Ni, ≤0.1% P and ≤0.02% S, and the balance is Fe and unavoidable impurities.
2. The Ni-containing ductile iron material according to claim 1, characterized in that: The Ni content is 1.43% to 8.07%.
3. A method for preparing the Ni-containing ductile iron material according to claim 1 or 2, characterized in that: The following steps are involved: S1: Rapidly cooling the molten iron containing Ni element after inoculation and spheroidization to the pseudo-eutectic region to obtain Ni-containing ductile iron or profiles; S2: homogenizing annealing the Ni-containing ductile iron or profile; S3: The ductile iron casting or profile after homogenization treatment is heated again and then tempered to obtain Ni-containing ductile iron material.
4. The method for preparing the Ni-containing ductile iron material according to claim 3, characterized in that: In S1, the rapid cooling rate is ≥50°C / s.
5. The method for preparing ductile iron material according to claim 3, characterized in that: In S2, the annealing method is: heating the ductile iron profile to 950-1050°C, keeping the temperature for 8-12 hours, and then taking it out of the furnace and air-cooling it to room temperature.
6. The method for preparing the Ni-containing ductile iron material according to any one of claims 3 to 5, characterized in that: In S3, the re-heating treatment is to heat the Ni-containing ductile iron casting or profile to 950°C, keep it at this temperature for 3 hours, and water quench it; the tempering treatment is to heat the Ni-containing ductile iron casting or profile to 500°C, keep it at this temperature for 2 hours, and air cool it.
7. The method for preparing the Ni-containing ductile iron material according to claim 3, characterized in that: The metal matrix structure of the ductile iron material is tempered martensite+residual austenite, and the material structure is tempered martensite+residual austenite+graphite nodules.
8. The method for preparing the Ni-containing ductile iron material according to claim 7, characterized in that: The density of the graphite ball is greater than 500 / mm 2 The ball diameter ranges from 25 to 40 μm, and the ball-ink spacing is 50 μm.