Smelting method of fine-grain rail steel
Through converter smelting, LF refining and continuous casting processes, combined with VD vacuum degassing and slow cooling treatment, the problems of taking into account both the strength and plastic toughness of high carbon rail materials were solved, and small-grain size rail steel with high strength and excellent plasticity were prepared.
Patent Information
- Application Number
- CN202411073429.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-26
AI Technical Summary
While the existing high-carbon rail materials increase their strength, the plastic toughness is reduced, making it difficult to take into account the strength and plastic toughness requirements of the rails.
Converter smelting, LF refining, RH refining and continuous casting process, strong deoxidation is performed by adding low aluminum silicon barium to control oxygen and aluminum content, combined with VD vacuum degassing and white slag refining, control alloy element components, and ensure the composition and temperature of molten steel. , fine-tuning and heating are performed, and finally a slow cooling treatment is performed to obtain an optimized grain size.
The prepared rail steel has good strength and plastic toughness, the inclusion level is controlled below level 2.5, and the grain size is greater than level 8, which has both high strength and excellent plasticity.
Smart Images

Figure CN119020671A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rail steel smelting and preparation, and in particular relates to a smelting method of fine-grain rail steel. Background Art
[0002] The development trend of my country's railways is high speed and heavy load. The development of heavy-load railways puts forward more stringent requirements on rails. Rails should not only have high strength and hardness to resist the contact wear between wheels and rails, but also have good plasticity and toughness to resist surface damage such as peeling, fatigue cracks and brittle fracture of rails. At present, the more commonly used rail composition is high carbon steel, and the corresponding organization type is pearlite organization. With the increase of strength, the plasticity and toughness of rails of this material decrease significantly. In order to improve the brittleness of rails caused by the increase of carbon content, it is necessary to ensure the plasticity and toughness of materials through alloy composition design, rolling and heat treatment process.
[0003] By adding alloy elements, controlling deformation parameters during rail rolling, and optimizing heat treatment, the grain size of the rail can be improved. In order to obtain rail products with fine grain size, the strength and plastic toughness of the rail are reasonably matched through composition design, rolling process control, and heat treatment process optimization. The present invention provides a composition design and smelting method for fine-grained rails. Summary of the invention
[0004] The object of the present invention is to provide a method for smelting fine-grained rail steel, so as to achieve the purpose of improving both the strength and the plasticity of the rail steel.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] The invention discloses a smelting method for fine-grained rail steel, wherein the smelting process of the rail steel comprises converter smelting, LF refining, RH refining and continuous casting processes, and is characterized in that after normal blowing of the molten iron in the furnace, no deoxidizer is added to the converter tapping, and when the tapping reaches 30%-60%, an aluminum-free deoxidizer is added for deoxidation and alloying, and 2-5kg of low-aluminum silicon calcium barium is added to strongly deoxidize the molten steel to ensure a low oxygen content and aluminum content in the molten steel; after the tapping is completed, 2-10kg / t of slag washing material containing Al2O3 is added, and the Al content in the steel is controlled at the same time; then the molten steel enters LF refining, active lime and wollastonite are added for white slag refining, and Ar blowing operation is performed throughout the ladle refining; desulfurization is performed according to the composition and temperature of the molten steel in the converter, the composition is finely adjusted and the temperature is increased, and alloy elements are added during the refining process to control the composition; the final slag basicity is controlled to be 2.9-3.1, wherein the Al2O3 content is below 10wt%, the white slag is maintained for more than 25min, and weak stirring is not required during the process;
[0007] Adopt VD vacuum degassing, vacuum degree ≤0.10KPa, deep vacuum time ≥15min; ensure soft blowing time ≥15min, molten steel standing time more than 20min, molten steel shall not be exposed during soft blowing. During the continuous casting process, the overheat degree of the continuous casting billet is controlled to be ΔT≤30℃, and the constant pulling speed is less than 0.68m / min; the billet is slowly cooled by heating at 500-600℃ for 24 hours, and then slowly cooled by stacking without heating for more than 24 hours;
[0008] The chemical composition range of the rail steel by mass percentage is: C content is 0.9-1.5%, Mn content is 0.6-1.1%, Si content is 0.4-1.0%, alloy content Cr+V+Nb+Cu+Ni≦0.6%, wherein the total Cr in the steel is required to be below 0.35%, the rest is V+Nb+Cu+Ni≦0.25%, and the balance is Fe and unavoidable impurities.
[0009] Furthermore, the final slag basicity is controlled to 3.0.
[0010] Furthermore, the casting process can achieve automatic liquid level control.
[0011] Furthermore, the specifications of the continuous casting billet are 280mm×380mm or 320mm×415mm.
[0012] Furthermore, the cut-to-length length of the steel billet is selected according to the length of the rolled rail.
[0013] Furthermore, the inclusion level of rail steel is well controlled, with the sum of A+B+C+D reaching below level 2.5.
[0014] Furthermore, the grain size of the rail steel is greater than grade 8.
[0015] Compared with the prior art, the beneficial technical effects of the present invention are:
[0016] The inclusion level of the rail steel prepared by the present invention is well controlled, the sum of A+B+C+D reaches below level 2.5, and the grain size is greater than level 8.
[0017] The rails have both excellent strength and plasticity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings.
[0019] Figure 1 Schematic diagram of the grain size microstructure of the fine-grained rail steel according to Example 1 of the present invention. DETAILED DESCRIPTION
[0020] On one hand, the present invention provides a smelting method of fine-grained rail steel, which includes converter smelting, LF refining, RH refining and continuous casting. In the method of the present invention, in order to control the inclusions in the steel, low aluminum silicon calcium barium is added in the converter smelting for strong deoxidation, the S content in the steel is reduced in the LF refining process, and then the VD vacuum treatment and soft blowing are used to control the composition of the molten steel to be fine-tuned to the target range.
[0021] The composition range for the casting machine after VD is as follows: C content is 0.9-1.5%, Mn content is 0.6-1.1%, Si content is 0.4-1.0%, and the alloy content Cr+V+Nb+Cu+Ni≦0.6%, of which the total Cr in the steel is required to be less than 0.35%, the rest is V+Nb+Cu+Ni≦0.25%, and the balance is Fe and unavoidable impurities.
[0022] According to the above-obtained 280mm*380mm rectangular ingot, the ingot was heated at 1250-1280℃ for 3 hours, deformed and rolled 13 times, and the final rolling temperature was controlled at 900-980℃, ensuring the rail heat treatment inlet temperature at 700-810℃ and the heat treatment outlet temperature at 400-550℃. The strength, hardness, inclusions and grain size of the rail were tested. The specific smelting process is shown in Table 1.
[0023] Table 1 Smelting process
[0024]
[0025] It can be seen from Table 1 that the inclusion level of rail steel is well controlled, and the sum of A+B+C+D is below level 2.5. Figure 1 , the grain size is greater than level 8 and reaches level 9.5.
[0026] Table 2 Mechanical properties of rails
[0027]
[0028] It can be seen that the high rail strength in Example 1 is due to the grain refinement and strengthening effect obtained by the method of the present invention, which ensures the plasticity of the rail.
[0029] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for smelting fine-grained rail steel, wherein the rail steel smelting process includes converter smelting, LF refining, RH refining and continuous casting steps, characterized in that: After the molten iron is blown normally, no deoxidizer is added to the converter tapping. When the tapping reaches 30%-60%, an aluminum-free deoxidizer is added for deoxidation and alloying. In addition, 2-5kg of low-aluminum silicon calcium barium is added to strongly deoxidize the molten steel to ensure a low oxygen content and aluminum content in the molten steel. After the tapping is completed, 2-10kg / t of Al2O3-containing slag washing material is added to control the Al content in the steel. After that, the molten steel enters the LF refining and active lime and wollastonite are added for white slag refining. Ar blowing is performed throughout the ladle refining process. Desulfurization is performed according to the composition and temperature of the converter molten steel, and the composition is fine-tuned and the temperature is increased. During the refining process, alloy elements are added to control the composition. The final slag basicity is controlled to be 2.9-3.1, wherein the Al2O3 content is below 10wt%, and the white slag is maintained for more than 25min. No weak stirring is required during the process. Adopt VD vacuum degassing, vacuum degree ≤0.10KPa, deep vacuum time ≥15min; ensure soft blowing time ≥15min, molten steel standing time more than 20min, molten steel shall not be exposed during soft blowing. During the continuous casting process, the overheat degree of the continuous casting billet is controlled to be ΔT≤30℃, and the constant pulling speed is less than 0.68m / min; the billet is slowly cooled by heating at 500-600℃ for 24 hours, and then slowly cooled by stacking without heating for more than 24 hours; The chemical composition range of the rail steel by mass percentage is: C content is 0.9-1.5%, Mn content is 0.6-1.1%, Si content is 0.4-1.0%, alloy content Cr+V+Nb+Cu+Ni≦0.6%, wherein the total Cr in the steel is required to be below 0.35%, the rest is V+Nb+Cu+Ni≦0.25%, and the balance is Fe and unavoidable impurities.
2. The smelting method of fine-grained rail steel according to claim 1, characterized in that: Control the final slag basicity to 3.
0.
3. The smelting method of fine-grained rail steel according to claim 1, characterized in that: The casting process can achieve automatic liquid level control.
4. The smelting method of fine-grained rail steel according to claim 1, characterized in that: The specifications of the continuous casting billet are 280mm×380mm or 320mm×415mm.
5. The smelting method of fine-grained rail steel according to claim 1, characterized in that: The cut length of the billet is selected according to the length of the rolled rail.
6. The smelting method of fine-grained rail steel according to claim 1, characterized in that: The inclusion level of the rail steel is well controlled, and the sum of A+B+C+D reaches below level 2.
5.
7. The smelting method of fine-grained rail steel according to claim 6, characterized in that: The rail steel grain size is greater than grade 8.
Citation Information
Patent Citations
Heavy load steel rail and producing method thereof
CN105177431A
Smelting method for reducing formation of large inclusions in steel rail for high-speed railway
CN112593136A
High-carbon microalloyed heat treatment steel rails and welding method thereof
CN112647024A
Perlite rail of high abrasion resistance and method of mfg. the same
CN1140473A
Superfine pearlite steel rail for heavy haul railway and production method of superfine pearlite steel rail
CN116695000A