Economical high-toughness engineering machinery steel with yield strength larger than or equal to 960 MPa and production method
By adjusting the chemical composition and heat treatment process, the production cost of 960MPa grade high-strength steel is reduced, the problems of high costs in the existing technology are solved, and high toughness and low-cost steel production for construction machinery are achieved.
Patent Information
- Application Number
- CN202410974182.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The production cost of existing 960MPa grade high-strength steel is relatively high, mainly due to the high alloy design cost due to the precious alloy elements Cr and Mo.
By adjusting chemical composition, the content of Cr and Mo is reduced, and different heat treatment processes are adopted, including controlling the heating temperature of the casting billet, rolling temperature and quenching and insulating time, replacing Ti and B to reduce production costs while maintaining or increasing yield strength, Tensile strength and elongation.
The production of high-toughness engineering machinery steel with a yield strength ≥960MPa, tensile strength ≥990MPa and elongation ≥13% is achieved, while reducing production costs by at least 5%.
Smart Images

Figure BDA0004954065840000051 
Figure BDA0004954065840000061 
Figure BDA0004954065840000062
Abstract
Description
Technical Field
[0001] The present invention relates to a steel for engineering machinery and a production method, in particular to an economical high-toughness steel for engineering machinery with a yield strength of ≥960MPa and a production method. Background Art
[0002] The engineering machinery industry uses a huge amount of 960MPa grade high-strength steel, such as excavator bucket linings and side panels, mining car compartment linings, etc. This grade of steel is generally designed with precious alloy elements such as Cr, Mo, Ni, etc., and is produced using a quenching and tempering process. This design idea results in a high alloy design cost. For example, after searching:
[0003] The document of Chinese patent application number CN201110098008.2 discloses "An ultra-high strength steel with a yield strength of 960 MPa and its production method", whose chemical composition by weight percentage is: C: 0.07-0.09%; Si: 0.15-0.25%; Mn: 1.00-1.20%; Cr: 1.05-1.15%; Mo: 0.15-0.20%; Al: 0.01-0.06%; P: ≤0.02 %; S: ≤0.01%; N: ≤0.008%; the rest is Fe and unavoidable impurities; the production method is: smelting, casting into ingot; heating to 1150~1250℃; final rolling temperature is 840~900℃; final cooling temperature is 640~700℃; quenching and tempering treatment, quenching heating temperature is 880~920℃, holding time is 20~60min, tempering heating temperature is 150~450℃, holding time is 90-180min. Although the steel plate meets the performance requirements of 960MPa ultra-high strength steel and has good elongation and impact toughness, it contains Cr: 1.05~1.15%; Mo: 0.15~0.20%, resulting in high production cost. Summary of the invention
[0004] The present invention aims to overcome the disadvantage of high production cost in the prior art, and to provide an economical high-toughness steel for engineering machinery with a yield strength of ≥960MPa and a production method, which ensures a yield strength of ≥960MPa, a tensile strength of ≥990MPa, an elongation of ≥13%, and a Kv2 of ≥70J at -40°C, and which can reduce the production cost by at least 5% compared with the prior art.
[0005] Measures to achieve the above objectives:
[0006] The invention discloses an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa, wherein the components and weight percentage contents thereof are as follows: C: 0.10-0.16%, Si≤0.1%, Mn: 0.7-1.2%, P≤0.015%, S≤0.010%, Als: 0.03-0.05%, Ti: 0.05-0.08%, B: 0.001-0.003%, and the rest are Fe and impurities.
[0007] Preferably, the weight percentage of Mn is 0.92-1.20%.
[0008] Preferably, the weight percentage content of Ti is 0.06-0.072%.
[0009] Preferably, the weight percentage content of B is 0.0017-0.0022%.
[0010] A method for producing an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa, comprising the following steps:
[0011] 1) Conventional smelting and continuous casting into billets;
[0012] 2) Heating the ingot: controlling the heating temperature of the ingot to be between 1220 and 1260°C;
[0013] 3) Perform rough rolling and control the end temperature of rough rolling to be between 1020°C and 1100°C;
[0014] 4) Perform finish rolling, control the starting rolling temperature not to exceed 1060°C, and the final rolling temperature to be between 820 and 920°C;
[0015] 5) Rapid cooling, cooling to the coiling temperature at a cooling rate of 60 to 120°C / S;
[0016] 6) Coil the steel sheet: control the coiling temperature at 520-660°C;
[0017] 7) After uncoiling, quenching treatment is performed: the quenching temperature is controlled at 810-920°C and kept at this temperature for 4-18 minutes;
[0018] 8) After being cut to a fixed length, the steel is tempered at a temperature of 460 to 620°C and a tempering time of 8 to 20 minutes;
[0019] 9) Reserved.
[0020] Preferably, the starting rolling temperature is between 960 and 1030°C, and the final rolling temperature is between 840 and 900°C.
[0021] Preferably, the cooling rate is 75-110°C / S.
[0022] Preferably, the coiling temperature is between 555 and 635°C.
[0023] Preferably, the quenching temperature is between 850°C and 910°C, and the quenching holding time is between 6 and 12 minutes.
[0024] Preferably, the tempering temperature is between 515 and 620°C.
[0025] Functions and mechanisms of each component and main process in the present invention
[0026] C: C is the cheapest element to improve material strength. As the carbon content increases, hardness and strength increase, but plasticity and welding performance decrease. If its content is less than 0.10%, it cannot meet the material strength requirements; if its content is greater than 0.16%, it affects welding performance and forming performance. Therefore, its content is limited to 0.10-0.16%.
[0027] Mn: Mn significantly reduces Ar1 temperature and austenite decomposition rate, improves the stability of supercooled austenite, promotes stress release of austenite, increases the residual austenite content in the final structure, and improves cold bending performance. However, if the Mn content is too high, it will increase temper brittleness and cause serious center segregation. Taking all factors into consideration, the Mn weight percentage should be 0.7-1.2%.
[0028] Si: Si can reduce the diffusion rate of carbon in ferrite, promote the formation of ferrite, and also deteriorate the surface quality. Taking all factors into consideration, the Si weight percentage is preferably 0 to 0.1%.
[0029] Als: Als can deoxidize steel, reduce the inclusion content, and also play a role in refining grains. Taking all factors into consideration, Als is between 0.03 and 0.05%.
[0030] Ti: Ti can combine with N to form stable TiN during the solidification process of steel, which can strongly hinder the migration of austenite grain boundaries, refine austenite grains, and provide a structural basis for refining the structure after heat treatment and improving the strength and toughness matching of steel. At the same time, the precipitation of nano-scale TiC precipitation phase during rolling and cooling can improve the strength of steel. Taking all factors into consideration, the weight percentage of Ti is preferably 0.05-0.08%.
[0031] P, S: P and S are harmful impurity elements in steel. P in steel is easy to form segregation in steel, reducing the toughness and welding performance of steel. S is easy to form plastic sulfide, causing stratification of steel plate and deteriorating the performance of steel plate. Therefore, the lower the P and S content, the better. Taking comprehensive consideration, the P and S content of steel is P≤0.015%, S≤0.010%.
[0032] B: B can greatly improve the hardenability, but when B is too much, it is easy to be enriched at the grain boundary, which will reduce the grain boundary binding energy, making the steel plate more inclined to fracture along the grain when subjected to impact load, and reducing the low-temperature impact work of the steel plate. Therefore, the addition amount of B in the present invention is 0.001-0.003%.
[0033] The reason why the heating temperature of the casting blank is controlled within the range of 1220-1260° C. is due to the homogenization of austenite and the sufficient diffusion of elements such as C and B.
[0034] The reason why the rough rolling end temperature is controlled at 1020-1100° C. in the present invention is that the growth of austenite after rough rolling is suppressed, thereby playing a role in refining the grains.
[0035] The reason why the start temperature of finishing rolling is controlled not to exceed 1060° C. and the final rolling temperature is controlled between 820° C. and 920° C. is to refine the organizational structure after finishing rolling.
[0036] The reason why the present invention controls the cooling rate to be 60-120°C / S is that the organization transformation is carried out quickly after the finish rolling, and the organization structure is refined at the same time.
[0037] The reason why the coiling temperature is controlled at 520-660° C. in the present invention is that the structure transformation and TiC precipitation are carried out quickly.
[0038] The reason why the quenching temperature is controlled at 810-920° C. and kept at this temperature for 4-18 minutes is to confiscate austenitization.
[0039] The reason why the tempering temperature is controlled at 460-620° C. and the tempering time is controlled at 8-20 minutes in the present invention is that the tempering transformation of the quenched martensite is carried out.
[0040] Compared with the prior art, the present invention ensures that the yield strength is ≥960MPa, the tensile strength is ≥990MPa, the elongation is ≥13%, and the -40°C Kv2 is ≥70J. Moreover, by replacing the expensive elements Cr and Mo originally added with Ti and B through component involvement, the production cost can be reduced by at least 5% compared with the prior art. DETAILED DESCRIPTION
[0041] The present invention is described in detail below:
[0042] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0043] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0044] Table 3 is a table of performance test results of various embodiments and comparative examples of the present invention.
[0045] Each embodiment of the present invention is produced according to the following steps
[0046] 1) Conventional smelting and continuous casting into billets;
[0047] 2) Heating the ingot: controlling the heating temperature of the ingot to be between 1220 and 1260°C;
[0048] 3) Perform rough rolling and control the end temperature of rough rolling to be between 1020°C and 1100°C;
[0049] 4) Perform finish rolling, control the starting rolling temperature not to exceed 1060°C, and the final rolling temperature to be between 820 and 920°C;
[0050] 5) Rapid cooling, cooling to the coiling temperature at a cooling rate of 60 to 120°C / S;
[0051] 6) Coil the steel sheet: control the coiling temperature at 520-660°C;
[0052] 7) After uncoiling, quenching treatment is performed: the quenching temperature is controlled at 810-920°C and kept at this temperature for 4-18 minutes;
[0053] 8) After being cut to a fixed length, the steel is tempered at a temperature of 460 to 620°C and a tempering time of 8 to 20 minutes;
[0054] 9) Reserved.
[0055] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0056]
[0057]
[0058] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0059]
[0060] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0061]
[0062]
[0063] It can be seen from Table 3 that the yield strength and tensile strength of a 960MPa grade low-cost, high-toughness high-strength steel for engineering machinery prepared in Examples 1-7 of the present invention are similar to those of Comparative Examples 1-2, but the elongation and -40°C Kv2 are significantly better than those of the comparative examples, especially the -40°C Kv2 is greater than 70J, which is much higher than that of the comparative examples, which shows that the products of Examples 1-7 have good low-temperature toughness; and the expensive elements originally added are replaced by Ti and B, so that the production cost can be reduced by at least 5% compared with the prior art.
[0064] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. An economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa, wherein the components and weight percentage contents are as follows: C: 0.10-0.16%, Si≤0.1%, Mn: 0.7-1.2%, P≤0.015%, S≤0.010%, Als: 0.03-0.05%, Ti: 0.05-0.08%, B: 0.001-0.003%, and the rest are Fe and impurities.
2. The economical high-toughness engineering machinery steel with a yield strength of ≥960 MPa as claimed in claim 1, characterized in that: The weight percentage of Mn is 0.92-1.20%.
3. The economical high-toughness engineering machinery steel with a yield strength of ≥960 MPa as claimed in claim 1, characterized in that: The weight percentage content of Ti is 0.06-0.072%.
4. The economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa as claimed in claim 1, characterized in that: The weight percentage content of B is 0.0017-0.0022%.
5. A method for producing an economical high-toughness engineering machinery steel with a yield strength of ≥960 MPa as claimed in claim 1, comprising the following steps: 1) Conventional smelting and continuous casting into billets; 2) Heating the ingot: controlling the heating temperature of the ingot to be between 1220 and 1260°C; 3) Perform rough rolling and control the end temperature of rough rolling to be between 1020°C and 1100°C; 4) Perform finish rolling, control the starting rolling temperature not to exceed 1060°C, and the final rolling temperature to be between 820 and 920°C; 5) Rapid cooling, cooling to the coiling temperature at a cooling rate of 60 to 120°C / S; 6) Coil the steel sheet: control the coiling temperature at 520-660°C; 7) After uncoiling, quenching treatment is performed: the quenching temperature is controlled at 810-920°C and kept at this temperature for 4-18 minutes; 8) After being cut to a fixed length, the steel is tempered at a temperature of 460 to 620°C and a tempering time of 8 to 20 minutes; 9) Reserved.
6. The method for producing an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa as claimed in claim 5, characterized in that: The starting rolling temperature is between 960 and 1030°C, and the final rolling temperature is between 840 and 900°C.
7. The method for producing an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa as claimed in claim 5, characterized in that: The cooling rate is 75-110°C / S.
8. The method for producing an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa as claimed in claim 5 is characterized by: The coiling temperature is between 555 and 635°C.
9. The method for producing an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa as claimed in claim 5 is characterized by: The quenching temperature is between 850 and 910°C, and the quenching holding time is between 6 and 12 minutes.
10. The method for producing an economical high-toughness steel for engineering machinery with a yield strength of ≥960 MPa as claimed in claim 5 is characterized by: The tempering temperature is between 515 and 620°C.
Citation Information
Patent Citations
Hot-rolled automobile steel with yield strength of higher than 960 MPa, and manufacturing method thereof
CN112877608A
Bainite non-quenched-and-tempered high-strength steel with tensile strength greater than or equal to 960 MPa and manufacturing method thereof
CN113373376A
Steel with yield strength of 900-1100 MPa for welded structure and production method
CN116904869A
High-strength hot-rolled steel sheet having excellent low temperature toughness and method for producing the same
JP2011052321A
High strength hot rolled steel sheet and production method therefor
JP2016204734A
Cited By
Method for improving surface quality of hot-rolled commercial wheel steel
CN120001798A
A method for improving the surface quality of hot-rolled commercial vehicle wheel steel
CN120001798B