Zinc-aluminum-magnesium steel suitable for photovoltaic shock absorber, preparation process of zinc-aluminum-magnesium steel and photovoltaic shock absorber

By applying zinc-aluminum-magnesium alloy layer on the metal surface, the compact oxide film is formed using the components of zinc, aluminum, magnesium and manganese, the problem of poor corrosion resistance of traditional anti-rust paint coating is solved, and the wear resistance of metal workpieces is improved and corrosion resistance, and reduce production costs and temperatures under sunlight.

CN118910529APending Publication Date: 2024-11-08ZHENGZHOU XSD IND CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410991965.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The use of anti-rust paint to apply metal workpieces in traditional processes has poor corrosion resistance and is prone to wear, and is difficult to produce and costly.

Method used

Using zinc, aluminum, magnesium steel and its preparation process, by applying zinc, aluminum, magnesium alloy layer on the metal surface, the addition of zinc, aluminum, magnesium components and manganese, a dense oxide film is formed to improve wear resistance and corrosion resistance. , and the yield rate is improved by first processing and molding and then applying zinc, magnesium, aluminum coating.

Benefits of technology

It significantly improves the wear resistance and corrosion resistance of metal workpieces, extends protection time, reduces production costs, and improves yield. The silver-white reflective effect of zinc, aluminum, magnesium steel reduces temperature in the sun, providing more Good protection effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910529A_ABST
    Figure CN118910529A_ABST
Patent Text Reader

Abstract

The invention relates to the field of coating and plating technologies, in particular to zinc-aluminum-magnesium steel suitable for a photovoltaic shock absorber, a preparation technology of the zinc-aluminum-magnesium steel and the photovoltaic shock absorber. 1-3 parts of magnesium; and 1-3 parts of zinc. A metal workpiece coated with the zinc-magnesium-aluminum coating prepared through the method has the effects of being higher in corrosion resistance and higher in wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coating technology, and in particular to a zinc-aluminum-magnesium steel suitable for a photovoltaic shock absorber, a preparation process thereof, and a photovoltaic shock absorber. Background Art

[0002] Zinc-aluminum-magnesium steel plate refers to a steel plate with a zinc-aluminum-magnesium coating. Steel plates with high corrosion resistance are often required in fields such as steel silos, hardware machinery, etc. The traditional technology is to galvanize the steel plate, which is called ultra-thick zinc-layer pure zinc steel plate. The ultra-thick zinc-layer pure zinc steel plate with a pure zinc layer thickness of 800g / m2 can have a service life of up to 30 years. However, the coating of ultra-thick zinc-layer pure zinc steel plates is usually prepared by hot dip plating, but the coating is too thick, which makes production difficult and costly. For zinc-aluminum-magnesium steel plates, the service life of a coating thickness of 275g / m2 can reach more than 30 years. The reduced coating thickness makes production less difficult, and the cost is lower than that of ultra-thick zinc-layer pure zinc steel plates. Summary of the invention

[0003] In order to solve the problem of poor corrosion resistance and easy wear caused by coating metal workpieces with anti-rust paint in traditional processes, the present application provides a zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers, a preparation process thereof, and a photovoltaic shock absorber.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions: A zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers, comprising the following components in parts by mass: 1-3 parts of aluminum; 1-3 parts of magnesium; 1-3 parts of zinc.

[0005] Through the above technical scheme, zinc-aluminum-magnesium steel is widely used as a coating material for metal surfaces. Due to its strong corrosion resistance, zinc-aluminum-magnesium steel can enhance the weather resistance of metal workpieces after being coated on the metal surface. Compared with the traditional protection method of coating anti-rust paint on the surface of metal workpieces, the use of zinc-magnesium-aluminum steel has stronger wear resistance, and reduces the corrosion of metal workpieces caused by damage to anti-rust paint. When zinc-magnesium-aluminum steel is damaged, the magnesium phase in the zinc-magnesium-aluminum steel will move to the damaged area to oxidize and form a dense oxide film, which continues to protect the metal workpiece, greatly extending the protection time. At the same time, zinc-magnesium-aluminum steel has a silvery-white metallic luster, which has better reflective effect than traditional dark anti-rust paint, making the temperature lower under the sun, and having a better effect of protecting the workpiece. In addition, zinc-magnesium-aluminum steel is a metal material with good ductility and plasticity, and can adapt to metal workpieces of various shapes.

[0006] In zinc-aluminum-magnesium alloy, zinc is a relatively active metal. When it comes into contact with steel plates, it forms a galvanic cell protection, which greatly slows down the corrosion rate of the steel plates. The aluminum and magnesium in the zinc-aluminum-magnesium steel plates form a dense oxide film covering the surface of the steel plates after being oxidized, isolating the steel plates from contact with oxidants, thereby slowing down the corrosion rate of the steel plates.

[0007] In the present invention, the zinc-aluminum-magnesium steel also includes a manganese component.

[0008] Through the above technical scheme, after many experiments by operators, it was found that after adding manganese components to zinc-magnesium-aluminum steel, the physical and chemical properties of zinc-magnesium-aluminum steel were significantly improved, especially the wear resistance was greatly improved. After adding metallic manganese to zinc-aluminum-magnesium steel, manganese played a role of phase change, which expanded the austenite zone of the metal material and increased the critical temperature, so that the metal material can still remain stable at high temperatures. At the same time, the addition of metallic manganese lowered the martensitic transformation temperature of the metal material and improved the hardenability of the metal material. At the same time, the addition of manganese made the mixing of the various metal phases of the alloy material more uniform, reducing the occurrence of aggregation.

[0009] In the present invention, the content of the manganese component is 0.5-5 parts.

[0010] Through the above technical solution, after many experiments by operators, it was found that when the manganese component in zinc-magnesium-aluminum steel is 0.5-5 parts When the zinc-magnesium-aluminum steel is heated and cooled, the physical and chemical properties of the steel are significantly improved, especially the wear resistance.

[0011] A method for preparing zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers comprises the following steps: S1: Put zinc, aluminum, magnesium, manganese and other components into a smelting furnace in proportion to melt and obtain hot dip solution; S2, annealing the steel plate, controlling the annealing temperature, and obtaining a steel matrix; S3, stamping the steel substrate obtained in step S2 according to demand to obtain a metal workpiece; S4, applying the hot dip solution obtained in step S1 to the steel substrate for hot dip plating, and performing secondary stamping after slightly cooling to obtain a metal workpiece coated with a zinc-aluminum-magnesium coating.

[0012] In the present invention, when the traditional process produces the zinc-magnesium-aluminum steel coated metal workpiece, the zinc-magnesium-aluminum hot dip liquid is generally applied on the steel plate, and then the coated steel plate is processed into the required workpiece. This method is easy to cause the zinc-magnesium-aluminum coating to be damaged when the coated steel plate is processed, resulting in a low yield rate. In the present technical solution, the metal workpiece is first processed and formed, and then the zinc-magnesium-aluminum coating is applied to the metal workpiece, and the zinc-magnesium-aluminum coating is slightly cooled to keep the zinc-magnesium-aluminum coating on the surface of the metal workpiece, and then a secondary stamping is performed to make the zinc-magnesium-aluminum coating fit closely with the metal workpiece, thereby improving the yield rate of the product.

[0013] In the present invention, the temperature of the hot dip liquid in step S1 is 400-600°C, and the temperature after cooling in step S1 is 200-400°C.

[0014] Through the above technical solution, operators have found through multiple experiments that the temperature of the hot dip liquid in step S1 is 400-600°C, and the temperature after cooling in step S1 is 200-400°C, which is more suitable for processing metal workpieces.

[0015] In the present invention, the hot-dip coating time in step S3 is 30-60 seconds.

[0016] Through the above technical solution, operators have found through multiple experiments that the hot-dip coating time in step S3 is more suitable for 30-60S. When the hot-dip coating time is too short, it is easy to cause incomplete coating of the zinc-magnesium-aluminum hot-dip solution.

[0017] A photovoltaic shock absorber comprises an oil storage cylinder, an oil storage cylinder cover is provided at one end of the oil storage cylinder, a working cylinder is coaxially provided in the oil storage cylinder, a connecting rod is coaxially slidably connected in the working cylinder, the connecting rod extends out of the oil storage cylinder in a direction away from the oil storage cylinder cover, a piston is provided at the end of the connecting rod close to the oil storage cylinder cover, the oil storage cylinder is coaxially covered with a dust cover, a dust cover is provided at the end of the dust cover away from the oil storage cylinder cover, a joint bearing is provided at the ends of the connecting rod and the oil storage cylinder cover away from each other, and the oil storage cylinder, the oil storage cylinder cover, the working cylinder, the connecting rod, the dust cover and the dust cover are all coated and modified with zinc-aluminum-magnesium steel.

[0018] Through the above technical scheme, the oil storage cylinder, oil storage cylinder cover, working cylinder and connecting rod are all coated and modified with zinc-aluminum-magnesium steel, making it less likely to be corroded during use, greatly improving the service life of the equipment, and a dust cover is mounted on the outer wall of the oil storage steel. One end of the dust cover is fixed with a dust cover cover. The dust cover plays a role in protecting the oil storage cylinder. Compared with the traditional method of applying anti-rust paint, the dust cover modified by zinc-aluminum-magnesium steel has a longer service life. At the same time, when the dust cover is corroded, the dust cover can be replaced instead of directly replacing the entire equipment, which is lower in cost.

[0019] In the present invention, a fixing ring is coaxially arranged on the inner side wall of the dust cover, and a limiting ring is coaxially arranged on one end of the dust cover toward the dust cover, and the limiting ring is arranged to be locked with the fixing ring.

[0020] Through the above technical solution, the limiting ring and the fixing ring are engaged to limit the dust cover, thereby reducing the occurrence of the dust cover being too inserted into the dust cover, thereby facilitating the disassembly and separation of the dust cover and the dust cover.

[0021] In the present invention, an indicator groove is coaxially provided on the outer wall of the dust cover, and the indicator groove corresponds to the position of the fixing ring.

[0022] With the above technical solution, the operator can conveniently observe the position of the fixing ring through the position of the indicator groove, thereby conveniently selecting a dust cover of a suitable size.

[0023] In the present invention, the dust cover and the dust cover cap are connected by a rolling process.

[0024] Through the above technical solution, the dust cover and the dust cover cover are connected by the rolling process, which is more convenient for connection and disassembly than the traditional welding process. The synthetic method of the present invention has the following beneficial effects: 1. Zinc-aluminum-magnesium steel is a coating material for metal surfaces. Due to its strong corrosion resistance, zinc-aluminum-magnesium steel can enhance the weather resistance of metal workpieces after being coated on the metal surface. 2. In this technical solution, the metal workpiece is first processed and formed, and then the zinc-magnesium-aluminum coating is applied to the metal workpiece, and the zinc-magnesium-aluminum coating is slightly cooled to keep the zinc-magnesium-aluminum coating on the surface of the metal workpiece, and then a secondary stamping is performed to make the zinc-magnesium-aluminum coating fit closely with the metal workpiece, thereby improving the yield rate of the product; 3. A dust cover is installed on the outer wall of the oil storage steel. One end of the dust cover is fixed with a dust cover cap. The dust cover plays a role in protecting the oil storage cylinder. Compared with the traditional method of applying anti-rust paint, the dust cover modified by zinc-aluminum-magnesium steel has a longer service life. At the same time, when the dust cover is corroded, the dust cover can be replaced instead of directly replacing the entire equipment, which is lower in cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a cross-sectional view of a photovoltaic shock absorber according to an embodiment of the present application.

[0026] Figure 2 It is a structural schematic diagram of a connection method of a dust cover and a dust cover cover of a photovoltaic shock absorber in an embodiment of the present application.

[0027] Explanation of the reference numerals: 1. Oil storage cylinder; 11. Oil storage cylinder cover; 2. Working cylinder; 3. Connecting rod; 31. Piston; 4. Dust cover; 41. Fixing ring; 42. Indicator groove; 5. Dust cover; 51. Limiting ring; 6. Spherical bearing. DETAILED DESCRIPTION

[0028] The present invention is further described below through specific implementation modes, but the protection scope of the present invention is not limited thereto.

[0029] The following is combined with Figure 1-2 This application is described in further detail.

[0030] The present application embodiment discloses a photovoltaic shock absorber, referring to Figure 1 as well as Figure 2 A photovoltaic shock absorber includes a cylindrical oil storage cylinder 1, one end of the oil storage cylinder 1 is opened and the opening is sealed by an oil storage steel cover, a working cylinder 2 is coaxially installed in the oil storage steel, a connecting rod 3 is coaxially slidably connected in the working cylinder 2, the connecting rod 3 extends out of the oil storage cylinder 1 in a direction away from the oil storage cylinder cover 11, and a piston 31 is fixed at one end of the connecting rod 3 close to the oil storage cylinder cover 11. When the connecting rod 3 is subjected to external force, the connecting rod 3 drives the piston 31 to move in the working cylinder 2, and the oil in the working cylinder 2 has a shock absorbing effect.

[0031] The oil storage cylinder 1 is coaxially covered with a cylindrical dust cover 4, and the end of the dust cover 4 away from the oil storage cylinder cover 11 is sealed by a dust cover cover, a fixing ring 41 is coaxially fixed on the inner wall of the dust cover 4, and an indicating groove 42 is coaxially opened on the outer wall of the dust cover 4, and the indicating groove 42 corresponds to the position of the fixing ring 41, and a limiting ring 51 is coaxially fixed to one end of the dust cover cover 5 facing the dust cover 4, and the limiting ring 51 is arranged to be in a locking position with the fixing ring 41, and the dust cover 4 and the dust cover cover 5 are connected by a rolling process.

[0032] Reference Figure 1 The ends of the connecting rod 3 and the oil storage cylinder cover 11 that are away from each other are both equipped with a spherical bearing 6 for connecting to other workpieces. The oil storage cylinder 1, the oil storage cylinder cover 11, the working cylinder 2, the connecting rod 3, the dust cover 4 and the dust cover cover 5 are all coated and modified with zinc-aluminum-magnesium steel.

[0033] The implementation principle of a photovoltaic shock absorber in an embodiment of the present application is as follows: the photovoltaic shock absorber is connected to other workpieces through the joint bearings 6 at both ends. When the joint bearings 6 are subjected to force, the force drives the piston 31 to move through the connecting rod 3. When the piston 31 moves in the working cylinder 2, the oil in the working cylinder 2 slows down the movement of the piston 31, thereby achieving a shock absorbing effect.

[0034] The oil storage cylinder 1, the oil storage cylinder cover 11, the working cylinder 2, and the connecting rod 3 are all coated and modified with zinc-aluminum-magnesium steel, making it less likely to corrode during use, greatly improving the service life of the equipment. A dust cover 4 is sleeved on the outer wall of the oil storage steel, and one end of the dust cover 4 is fixed with a dust cover cover 5. The dust cover 4 protects the oil storage cylinder 1 and reduces the dust in the air from entering the oil storage cylinder 1 and the working cylinder 2. The dust cover 4 and the dust cover cover 5 are modified by coating with zinc-aluminum-magnesium steel. Compared with the traditional method of applying anti-rust paint, the dust cover 4 modified by coating with zinc-aluminum-magnesium steel has a longer service life. At the same time, when the dust cover 4 is corroded, the dust cover 4 can be replaced instead of directly replacing the entire equipment, which is lower in cost.

[0035] The dust cover 4 and the dust cover cap 5 are connected by a rolling process, which causes less damage to the zinc-aluminum-magnesium coating compared to the traditional welding process, thereby making the corrosion resistance of the equipment longer.

[0036] The present application is further described in detail below in conjunction with various embodiments and comparative examples.

[0037] Embodiment 1: Each zinc-magnesium-aluminum coating is prepared by the following components in parts by mass:

[0038] The difference between Examples 2-5 and Comparative Examples 1-6 and Example 1 is that the components of the zinc-magnesium-aluminum coating are different, as shown in the following table: Aluminum (parts) Magnesium (part) Zinc (part) Manganese (parts) Example 1 2 1 3 0.2 Example 2 2 1 3 0.1 Example 3 2 1 3 0.5 Example 4 2 2 2 0.2 Example 5 2 3 1 0.2 Example 6 3 1 2 0.2 Comparative Example 1 2 1 3 0 Comparative Example 2 2 1 2 0.05 Comparative Example 3 2 1 3 0.8 Comparative Example 4 4 1 1 0.2 Comparative Example 5 1 4 1 0.2 Comparative Example 6 1 1 4 0.2 The difference between Comparative Example 7 and Example 1 is that the metal workpiece coated with the zinc-magnesium-aluminum coating is prepared using a traditional process, and the steps are as follows: S1: Put zinc, aluminum, magnesium, manganese and other components into a smelting furnace in proportion to melt and obtain hot dip solution; S2, annealing the steel plate, controlling the annealing temperature, and obtaining a steel matrix; S3, applying the hot dip solution obtained in step S1 to the steel substrate for hot dip plating to obtain a zinc-aluminum-magnesium coated steel plate; S4. The zinc-aluminum-magnesium coated steel sheet obtained in step S2 is stamped and formed according to demand.

[0039] The difference between Comparative Example 8 and Example 1 is that Comparative Example 8 is a metal workpiece coated with a traditional anti-rust paint.

[0040] Detection Methods After the zinc-magnesium-aluminum coatings prepared in the embodiments and comparative examples were applied to the surface of metal workpieces, various performance tests were performed.

[0041] Heat resistance Each metal workpiece was placed in an open sunny place at 12 noon for 2 hours to test the surface temperature of each metal workpiece.

[0042] Wear resistance Each metal workpiece was ground for 30 seconds using a 2000-grit grinding wheel, and the degree of wear of each metal workpiece was observed.

[0043] Corrosion resistance Each metal workpiece was placed in a sealed box, and salt spray was delivered into the box. The workpieces were kept for 6 hours, 24 hours, and 48 hours, respectively, and the degree of corrosion was observed. The degree of corrosion was scored on a scale of 0-10, with the higher the score, the greater the degree of corrosion.

[0044] The salt spray test adopts the standard: Salt spray test (IOS 9227, JIS Z2371, ASTM B117) 5% NaCL, 35℃.

[0045] Destructive test: Use a tool to make two scratches on the zinc-aluminum-magnesium coating on the surface of each metal workpiece. One scratch completely destroys the zinc-aluminum-magnesium coating to expose the metal workpiece, and the other scratch partially destroys the zinc-aluminum-magnesium coating. Then, each metal workpiece is tested for corrosion resistance.

[0046] The test results are shown in the following table: Example 1 Comparative Example 8 Surface temperature(℃) 26.2 35.1 Conclusion: It can be seen from the data of Example 1 and Comparative Example 8 in the above table that the surface temperature of the metal workpiece coated with the zinc-magnesium-aluminum coating prepared in the present application is lower under long-term exposure to the sun, which plays a good role in protecting the equipment. This is because the zinc-magnesium-aluminum steel has a silvery-white metallic luster, which has a better reflective effect than the traditional dark anti-rust paint, and the traditional dark anti-rust paint is more likely to absorb heat in the sun, which makes the temperature of the metal workpiece coated with the zinc-aluminum-magnesium coating lower in the sun, which reduces the damage of high temperature to the electronic components in the metal workpiece. Example 1 Comparative Example 7 Yield rate (%) 95.8 81.2

[0047] Conclusion: It can be seen from the data of Example 1 and Comparative Example 7 in the above table that the preparation process of the present application has a higher yield rate than the traditional process. This is because when the traditional process produces zinc-magnesium-aluminum steel coated metal workpieces, it is generally adopted to apply zinc-magnesium-aluminum hot dip liquid on the steel plate, and then the coated steel plate is processed into the required workpiece. When processing the coated steel plate, this method is likely to cause damage to the zinc-magnesium-aluminum coating at the bending part of the steel plate, resulting in a low yield rate. In the present technical solution, the metal workpiece is first processed and formed, and then the zinc-magnesium-aluminum coating is applied to the metal workpiece, which is slightly cooled to keep the zinc-magnesium-aluminum coating on the surface of the metal workpiece, and then a secondary stamping is performed to make the zinc-magnesium-aluminum coating fit closely to the metal workpiece, thereby reducing the damage to the zinc-aluminum-magnesium coating when the steel plate is bent, thereby improving the yield rate of the product. Degree of wear Example 1 More obvious Example 2 More obvious Example 3 Minor wear Comparative Example 1 Exposing metal workpiece Comparative Example 2 obvious Comparative Example 3 Minor wear

[0048] Conclusion: It can be seen from the data of Examples 1-3 and Comparative Examples 1-3 in the above table that in the present application, after manganese is added to the zinc-magnesium-aluminum coating, the wear resistance is greatly improved. This is because after adding metallic manganese to the zinc-aluminum-magnesium steel, manganese plays a role of phase change, which expands the austenite region of the metal material and increases the critical temperature, so that the metal material can still remain stable at high temperatures. At the same time, the addition of metallic manganese reduces the martensitic transformation temperature of the metal material and improves the hardenability of the metal material. At the same time, the addition of manganese makes the mixing of the various metal phases of the alloy material more uniform, reduces the occurrence of aggregation, and thus improves the overall wear resistance of the zinc-aluminum-magnesium coating. When the manganese component is 0.05-0.5 parts, the improvement in wear resistance is more obvious. When the component is greater than 0.5, the effect of continuing to add manganese is not significant. Therefore, it is more appropriate for the metallic manganese component added in the present application when synthesizing the zinc-aluminum-magnesium coating to be 0.05-0.5. 6h 24h 48h Example 1 0 1 3 Example 4 0 2 4 Example 5 0 2 4 Example 6 1 3 5 Comparative Example 4 3 4 7 Comparative Example 5 3 5 7 Comparative Example 6 4 5 8

[0049] Conclusion: It can be seen from the data of Examples 1, 4, 5, 6 and Comparative Examples 4-6 in the above table that the zinc-magnesium-aluminum coating in the present application, which is prepared according to the components of 1-3 parts of aluminum, 1-3 parts of magnesium and 1-3 parts of zinc, has good corrosion resistance. When the ratio of aluminum: magnesium: zinc is 2: 1: 3, the corrosion resistance of the zinc-magnesium-aluminum coating reaches the highest, which is the most preferred for the present application. When the components of aluminum, magnesium and zinc are respectively greater than 3 parts, the corrosion resistance of the zinc-magnesium-aluminum coating decreases significantly. This is because zinc, as a relatively active metal in the zinc-aluminum-magnesium alloy, forms a primary battery protection when it contacts the steel plate, which greatly slows down the corrosion rate of the steel plate, while the aluminum and magnesium in the zinc-aluminum-magnesium steel plate After being oxidized, a dense oxide film is formed to cover the surface of the steel plate, isolating the steel plate from contact with the oxidant, thereby slowing down the corrosion rate of the steel plate. When the zinc content is too high, the oxide film formed after the oxidation of metal aluminum and metal magnesium is small, and it is difficult to cover the entire surface of the zinc-aluminum-magnesium coating, making the oxidation rate of metal zinc too fast, resulting in a shorter overall corrosion resistance time of the zinc-aluminum-magnesium coating. When there are too many metal aluminum and metal magnesium, although a dense protective film will be formed, the current air pollution is serious. When facing acid rain with a low pH, aluminum oxide will react to destroy the oxide film, which reduces the corrosion resistance of the metal workpiece. Therefore, a suitable ratio of metal zinc, aluminum, and magnesium is required to make the prepared zinc-aluminum-magnesium coating have better corrosion resistance.

[0050] Conclusion: It can be seen from the data of Example 1 and Comparative Example 8 in the above table that after the zinc-aluminum-magnesium coating prepared in the present application is coated on the surface of a metal workpiece, when the zinc-aluminum-magnesium coating is damaged, it can still maintain a long corrosion resistance effect. In the prior art, anti-rust paint is used to protect metal workpieces. When the anti-rust paint is damaged, the metal workpiece is corroded more seriously. This is because when the zinc-magnesium-aluminum steel is damaged, the magnesium phase in the zinc-magnesium-aluminum steel will move to the damaged area to oxidize and form a dense oxide film, which continues to protect the metal workpiece, greatly extending the protection time. Traditional anti-rust paint does not have this function. Therefore, the zinc-aluminum-magnesium coating prepared in the present application has a stronger corrosion resistance effect.

[0051] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers, characterized in that: The composition comprises the following components in parts by weight: 1-3 parts of aluminum; 1-3 parts of magnesium; 1-3 parts of zinc.

2. The zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers according to claim 1, characterized in that: The zinc-aluminum-magnesium steel also includes a manganese component.

3. The zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers according to claim 2, characterized in that: The content of the manganese component is 0.05-0.5 parts.

4. A method for preparing zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers as described in claims 1-3, characterized in that: The steps include: S1: Put zinc, aluminum, magnesium, manganese and other components into a smelting furnace in proportion to melt and obtain hot dip solution; S2, annealing the steel plate, controlling the annealing temperature, and obtaining a steel matrix; S3, stamping the steel substrate obtained in step S2 according to demand to obtain a metal workpiece; S4, applying the hot dip solution obtained in step S1 to the steel substrate for hot dip plating, and performing secondary stamping after slightly cooling to obtain a metal workpiece coated with a zinc-aluminum-magnesium coating.

5. The method for preparing zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers according to claim 3, characterized in that: The temperature of the hot dip liquid in step S1 is 400-600°C, and the temperature after cooling in step S1 is 200-400°C.

6. The method for preparing zinc-aluminum-magnesium steel suitable for photovoltaic shock absorbers according to claim 3, characterized in that: The hot-dip coating time in step S3 is 30-60 seconds.

7. A photovoltaic shock absorber coated with zinc-aluminum-magnesium steel prepared as claimed in any one of claims 4 to 6, characterized in that: The invention comprises an oil storage cylinder (1), one end of which is provided with an oil storage cylinder cover (11), a working cylinder (2) is coaxially provided inside the oil storage cylinder (1), a connecting rod (3) is coaxially slidably connected inside the working cylinder (2), the connecting rod (3) extends out of the oil storage cylinder (1) in a direction away from the oil storage cylinder cover (11), the end of the connecting rod (3) close to the oil storage cylinder cover (11) is provided with a piston (31), the oil storage cylinder (1) is coaxially covered with a dust cover (4), the end of the dust cover (4) away from the oil storage cylinder cover (11) is provided with a dust cover, the ends of the connecting rod (3) and the oil storage cylinder cover (11) away from each other are both provided with a joint bearing (6), and the oil storage cylinder (1), the oil storage cylinder cover (11), the working cylinder (2), the connecting rod (3), the dust cover (4) and the dust cover cover (5) are all made of zinc-aluminum-magnesium steel.

8. A photovoltaic shock absorber according to claim 7, characterized in that: A fixing ring (41) is coaxially provided on the inner side wall of the dust cover (4), and a limiting ring (51) is coaxially provided on one end of the dust cover cover (5) facing the dust cover (4), wherein the limiting ring (51) is arranged in a locking position with the fixing ring (41).

9. A photovoltaic shock absorber according to claim 8, characterized in that: An indicator groove (42) is coaxially provided on the outer wall of the dust cover (4), and the indicator groove (42) corresponds to the position of the fixing ring (41).

10. A photovoltaic shock absorber according to claim 9, characterized in that: The dust cover (4) and the dust cover cap (5) are connected by a rolling process.

Citation Information

Cited By

  • Zinc-aluminum-magnesium steel suitable for photovoltaic shock absorber, manufacturing process therefor, and photovoltaic shock absorber

    WO2026021504A1