Transition layer design and preparation method based on slicing method
By designing and preparing alternating transition layers of Ti and TiN layers by slice method on the surface of titanium alloy, the problem of poor binding strength of TiN coating on the surface of titanium alloy is solved, the film-based binding force is improved and the preparation cost is reduced, and it is suitable for other hard The problem of poor bonding strength of the quality coating.
Patent Information
- Application Number
- CN202410991729.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The TiN coating bonding strength on the surface of titanium alloy is poor, mainly due to the excessive stress in the film-based bonding interface caused by the low hardness and large hardness gradient of titanium alloy. The existing research methods are complex and costly.
Using the transition layer design and preparation method based on the 'slicing method', the Ti layer and TiN layer are alternately plated on the titanium alloy substrate by ion plating to form a transition layer with performance gradient distribution, reducing the internal stress of the film base bonding interface and improving Membrane-based binding force.
It effectively improves membrane-based binding force, simplifies the preparation process, reduces costs, and is suitable for alloy surfaces with other similar characteristics, extending the service life of the parts.
Smart Images

Figure CN118910551A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ion plating preparation, and in particular relates to a transition layer design and preparation method based on a "slicing method". Background Art
[0002] TiN material plays an important role in reducing the adhesion of the tool during the cutting process due to its high melting point and high hardness. At the same time, its good wear resistance, corrosion resistance and high temperature stability make it widely used in the performance optimization of parts in the aerospace field.
[0003] At present, the main substrate materials used for TiN coatings include cemented carbide (CN117210735A), high-speed steel, bearing steel, etc. With the increasing demand for lightweight weapons and equipment in the aerospace field, the demand for surface modification of titanium and titanium alloys has increased sharply. Currently, there are few studies on TiN coatings on the surface of titanium and titanium alloys, and the effect is poor (CN115725942A). An important factor is that the bonding strength of TiN on the surface of titanium alloys is poor.
[0004] An important reason that affects the bonding strength of TiN coating on the surface of titanium alloy is that the hardness of titanium alloy is relatively low, with a value of 300HV~350HV, which is about 1 / 7 of TiN. The high hardness gradient leads to excessive internal stress at the film-substrate bonding interface; in addition, the large difference in linear expansion coefficient will also increase the stress at the interface, and the lattice mismatch will also aggravate the film-substrate interface stress, which is manifested as poor bonding strength on a macro scale. In response to such problems, current research mainly focuses on adding one or more specific materials, such as Ti, Cr, CrN, etc. as transition layers. This idea can certainly obtain a coating with high bonding strength, but it often requires multiple experiments to try the effects of various process parameters on bonding performance. The same coating between substrates of different materials needs to repeat the complete development process, which is relatively complicated and has high experimental costs. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a transition layer design and preparation method based on the "slicing method" in view of the deficiencies of the above-mentioned prior art. The method is based on the idea of the "slicing method", and adopts an ion plating method to prepare a transition layer consisting of a Ti layer and a TiN layer alternating in sequence on a titanium alloy substrate, and designs the structure of the Ti layer and the TiN layer layer layer by layer, and prepares a transition layer with a gradient performance distribution between the titanium alloy substrate and the TiN surface layer, thereby improving the film-substrate bonding strength and avoiding the problem of excessive internal stress at the film-substrate bonding interface caused by excessive differences in film-substrate performance, especially hardness performance, resulting in too low a film-substrate bonding strength.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a transition layer design and preparation method based on the "slicing method", characterized in that the method comprises the following steps:
[0007] Step 1: After grinding, polishing, rust removal, cleaning, degreasing, and drying, the titanium alloy is placed in a vacuum furnace of an ion plating device as a substrate;
[0008] Step 2: sandblast the target surface of the Ti target, and do not sandblast the back surface, and install it on the target base of the ion plating equipment after wiping and drying;
[0009] Step 3, connecting the ion plating equipment to argon and nitrogen, then turning on the ion plating equipment to heat and evacuate, and then filling with argon to perform glow cleaning on the titanium alloy substrate;
[0010] Step 4: Adjust the argon gas flow rate to bombard and clean the titanium alloy substrate and Ti target after glow cleaning in the ion plating equipment;
[0011] Step 5: Ti layers and TiN layers are alternately plated on the titanium alloy substrate after bombardment and cleaning in step 4 by ion plating, wherein each Ti layer is composed of a plurality of Ti layer units, and the coating time of a single Ti layer unit is T Ti Each TiN layer consists of several TiN layer units, and the coating time of a single TiN layer unit is T TiN , and the plating time of each Ti layer and TiN layer is alternately nT in the direction from the cleaned titanium alloy substrate to the surface. Ti , 1T TiN , (n-1)T Ti , 2T TiN , ..., 1T Ti , nT TiN , n is a natural number greater than 3, and a transition layer is formed on the titanium alloy substrate;
[0012] Step six: coating a TiN surface layer on the transition layer on the titanium alloy substrate in step five.
[0013] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that the grinding and polishing process in step one is: the titanium alloy is grinded with sandpaper #240, #400, #800, #1200, #1500, #2000, and #3000 in sequence, and then polished with diamond spray polishing agent with specifications of 0.5μm and 0.1μm respectively; the cleaning adopts anhydrous ethanol ultrasonic for 20 minutes.
[0014] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that the mass purity of the Ti target in step 2 is above 99.99%; the mass purity of the argon gas and the nitrogen in step 3 is above 99.99%, and the ion plating equipment is turned on and heated to 250°C, and the vacuum chamber background is evacuated to 5×10 -3Pa, and then filled with argon gas to a vacuum degree of 2×10 0 Pa, glow cleaning was performed for 15 min at a bias voltage of -1000 V, a duty cycle of 80%, and a temperature of 250°C.
[0015] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that in step 4, the argon gas flow rate is adjusted to a vacuum degree of 3×10 -1 Pa, bombardment cleaning was carried out for 5 min at a bombardment bias of -400 V, a bombardment current of 65 A, a duty cycle of 80%, and a temperature of 250°C.
[0016] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that the coating conditions of the single Ti layer unit in step 5 are: continuous argon gas flow, maintaining a working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150V, arc current to 60A, duty cycle to 80%, temperature to 250℃, coating time to T Ti The plating conditions of the single TiN layer unit are: maintaining the working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150V, fill with nitrogen to a flow ratio of N2:Ar=7:1, arc current 60A, duty cycle 80%, temperature 250℃, coating time T TiN .
[0017] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that the value of n in step five is 3, 4, 5 or 6. Under the condition that the substrate and the TiN surface layer remain unchanged, as the value of n increases, the more Ti layers and TiN layers in the transition layer, the smaller the hardness gradient, the smaller the stress generated, and the stronger the macroscopic bonding strength; but at the same time, there is a matching relationship between the thickness of the transition layer and the thickness of the TiN surface layer, so the thickness is not the thicker the better. The above-mentioned preferred value of n can achieve a good match between the two, and reduce the preparation cost and shorten the process flow under the premise of ensuring the improvement of the film-substrate bonding force. In addition, when the thickness of the TiN surface layer changes, the performance gradient distribution of the transition layer can be adjusted by adjusting the value of n to ensure the effect of the transition layer on improving the film-substrate bonding force.
[0018] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that in step 5, from the (n+n 2 ) / 2 layer units later, the time length between each adjacent layer unit is (T Ti +T TiN) / 2, and then complete the subsequent plating in sequence. From the direction from the titanium alloy substrate to the surface, as each layer unit increases, the Ti layer plating time decreases, that is, the number of Ti layers and thickness decrease, while the TiN layer plating time increases, that is, the number of TiN layers and thickness increase. By increasing the time (T Ti +T TiN ) / 2, continuous plating of the same coating is likely to cause grain growth in the organization. Re-preparing each layer unit after an interval is equivalent to starting to prepare each layer unit again. The grain size in the layer unit will be smaller, and the number of grain boundaries will increase, which will play a role in fine grain strengthening, avoiding the grain growth in each layer unit affecting the layer unit performance of the Ti layer and TiN layer, thereby ensuring that the performance of the transition layer is gradient distributed, which is beneficial to ensuring the effect of the transition layer on improving the film-substrate bonding strength.
[0019] The above-mentioned transition layer design and preparation method based on the "slicing method" is characterized in that the coating conditions of the TiN surface layer in step 6 are: maintaining a working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150 V, arc current to 65 A, gas flow ratio N2:Ar = 7:1, temperature to 250 °C, and coating time to 40 min.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] 1. The present invention is based on the concept of "slicing method", that is, according to the main elements of the matrix and the surface layer composition, the matrix is first cut into thin slices by "slicing method", and the fundamental cause of the large film-substrate internal stress is optimized and reorganized to obtain a transition layer with a step-by-step performance gradient. An ion plating method is used to prepare a transition layer composed of Ti layers and TiN layers alternating in sequence on a titanium alloy matrix, and the structures of the Ti layers and the TiN layers are designed layer by layer, so that from the titanium alloy matrix to the surface, the thickness of each Ti layer decreases successively, and the thickness of each TiN layer increases successively, and a transition layer with gradient performance distribution is prepared between the titanium alloy matrix and the TiN surface layer, thereby avoiding the problem of excessive internal stress at the membrane-substrate bonding interface caused by excessive difference in membrane-substrate properties, especially hardness properties, resulting in low membrane-substrate bonding force.
[0022] 2. The present invention designs the structure of the transition layer based on the "slicing method" concept, and controls the thickness of the Ti layer and TiN layer in the transition layer by controlling the plating time of the two layers. The control method is simple, with less interference, and it is easy to achieve precise control of the structure of each layer in the transition layer.
[0023] 3. The present invention adds an intermittent process during the plating process to avoid grain growth affecting the layer unit performance of the Ti layer and the TiN layer, thereby ensuring that the performance of the transition layer is gradient distributed, which is beneficial to ensuring the effect of the transition layer on improving the film-substrate bonding strength.
[0024] 4. The Ti layer and the TiN layer in the transition layer structure of the present invention correspond to the main components of the substrate and the coating, respectively, and no additional components or materials need to be added, thus avoiding the experimental process of redeveloping process parameters, simplifying the preparation process, and reducing the preparation cost.
[0025] 5. The transition layer structure design method of the present invention fundamentally solves the problem of poor bonding caused by excessive performance differences between the substrate and the coating. It is universal and can be widely used to systematically solve the problem of poor bonding of hard coatings on the surface of general titanium alloys or other alloys with similar characteristics, thereby extending the service life of parts.
[0026] 6. The transition layer structure design and preparation method of the present invention solves the problem of poor bonding when a hard coating is plated on a softer substrate surface. It is not only applicable to titanium alloy substrates and TiN coatings, but can also be extended to situations where the performance (such as hardness difference) of other substrates and target coatings is greatly different.
[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the transition layer design structure based on the "slicing method" of the present invention. DETAILED DESCRIPTION
[0029] Example 1
[0030] This embodiment includes the following steps:
[0031] Step 1: Grind and remove rust from TC6 titanium alloy using sandpaper of #240, #400, #800, #1200, #1500, #2000, and #3000 in sequence, then polish with diamond spray polishing agent with specifications of 0.5 μm and 0.1 μm, then use anhydrous ethanol ultrasonic cleaning for 20 minutes to remove oil, and then hang in a vacuum furnace of an ion plating equipment as a substrate after drying;
[0032] Step 2: sandblast the target surface of the Ti target with a mass purity of more than 99.99%, and do not sandblast the back surface. After wiping and drying, install it on the target base of the ion plating equipment;
[0033] Step 3: Connect the ion plating equipment to argon and nitrogen with a purity of more than 99.99%, then turn on the ion plating equipment, heat it to 250°C, and evacuate the vacuum chamber to 5×10 -3 Pa, and then filled with argon gas to a vacuum degree of 2×10 0 Pa, glow cleaning was performed for 15 min at a bias voltage of -1000 V, a duty cycle of 80%, and a temperature of 250 °C;
[0034] Step 4: Adjust the argon flow rate to a vacuum degree of 3×10 -1 Pa, bombarding and cleaning the TC6 titanium alloy substrate and Ti target in the ion plating equipment for 5 min at a bombardment bias of -400 V, a bombardment current of 65 A, a duty cycle of 80%, and a temperature of 250 °C;
[0035] Step 5: Ti layers and TiN layers are alternately plated on the TC6 titanium alloy substrate cleaned in step 4 by ion plating, wherein each Ti layer is composed of a plurality of Ti layer units, and the coating time of a single Ti layer unit is T Ti = 30s, the coating conditions of a single Ti layer unit are: continuous argon flow, maintaining the working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150V, arc current to 60A, duty cycle to 80%, temperature to 250℃, each TiN layer consists of several TiN layer units, and the coating time of a single TiN layer unit is T TiN = 30s, the coating conditions of a single TiN layer unit are: maintain the working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150V, fill with nitrogen to a flow ratio of N2:Ar=7:1, arc current 60A, duty cycle 80%, temperature 250℃, such as Figure 1 As shown, according to the direction from the cleaned TC6 titanium alloy to the surface, the plating time of each Ti layer and TiN layer is alternately 3T Ti , 1T TiN , 2T Ti , 2T TiN , 1T Ti , 3T TiN , and after the 6th layer unit, a 30-second pause is added between each adjacent layer unit, that is, the arc power supply is turned off for 30 seconds, and then subsequent plating is completed in sequence to form a transition layer on the TC6 titanium alloy;
[0036] Step 6: In step 5, a TiN surface layer is plated on the transition layer on the TC6 titanium alloy substrate; the plating conditions for the TiN surface layer are: maintaining a working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150 V, arc current to 65 A, gas flow ratio N2:Ar = 7:1, temperature to 250 °C, and coating time to 40 min.
[0037] According to the test, the bonding force between the TC6 titanium alloy substrate and the TiN surface layer in this embodiment is 62.52N.
[0038] Example 2
[0039] The difference between this embodiment and embodiment 1 is that in step 5, the plating time of each Ti layer and TiN layer is alternately 5T in the direction from the cleaned TC6 titanium alloy substrate to the surface. Ti , 1T TiN , 4T Ti , 2T TiN , 3T Ti , 3T TiN , 2T Ti , 4T TiN , 1T Ti , 5T TiN , and after the 30th layer unit, an interval of 30 seconds is added between each adjacent layer unit, that is, the arc power is turned off for 30 seconds, and then the subsequent plating is completed in sequence to form a transition layer on the TC6 titanium alloy substrate.
[0040] According to the test, the bonding force between the TC6 titanium alloy substrate and the TiN surface layer in this embodiment is 73.73N.
[0041] Comparative Example 1
[0042] The difference between this comparative example and Example 1 is that in step 5, a TiN surface layer is directly plated on the TC6 titanium alloy substrate cleaned in step 4 by ion plating; the plating conditions of the TiN surface layer are: maintaining a working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150 V, arc current to 65 A, gas flow ratio N2:Ar = 7:1, temperature to 250 °C, duty cycle to 80%, and coating time to 40 min.
[0043] After testing, the bonding force between the TC6 titanium alloy substrate and the TiN surface layer in this comparative example is 28.4N.
[0044] By comparing the comparative example 1 of the present invention with embodiments 1 to 2, it can be seen that, compared with comparative example 1, the transition layer structure prepared between the titanium alloy substrate and the TiN surface layer based on the "slicing method" in embodiments 1 to 2 greatly improves the film-substrate bonding strength; at the same time, the more the number of coating layers of the Ti layer and the TiN layer, the greater the film-substrate bonding strength.
[0045] Comparative Example 2
[0046] The difference between this comparative example and Example 1 is that the process of alternately plating the Ti layer and the TiN layer by ion plating in step 5 is continuous plating without pause.
[0047] After testing, the bonding force between the TC6 titanium alloy substrate and the TiN surface layer in this comparative example is 47.6N.
[0048] By comparing comparative example 2 of the present invention with example 1, it can be seen that the present invention avoids grain growth affecting the layer unit performance of the Ti layer and the TiN layer by adding an intermittent process during the plating process, thereby ensuring that the performance of the transition layer is gradiently distributed, which is beneficial to ensuring the effect of the transition layer on improving the film-substrate bonding strength.
[0049] Example 3
[0050] The difference between this embodiment and embodiment 1 is that the substrate used in step 1 is TC4 titanium alloy.
[0051] According to the test, the bonding force between the TC4 titanium alloy substrate and the TiN surface layer in this embodiment is 69.01N.
[0052] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A transition layer design and preparation method based on the "slicing method", characterized in that: The method comprises the following steps: Step 1: After grinding, polishing, rust removal, cleaning, degreasing and drying, the titanium alloy is placed in a vacuum furnace of an ion plating device as a substrate; Step 2: sandblast the target surface of the Ti target, and do not sandblast the back surface, and install it on the target base of the ion plating equipment after wiping and drying; Step 3, connecting the ion plating equipment to argon and nitrogen, then turning on the ion plating equipment to heat and evacuate, and then filling with argon to perform glow cleaning on the titanium alloy substrate; Step 4: Adjust the argon gas flow rate to bombard and clean the titanium alloy substrate and Ti target after glow cleaning in the ion plating equipment; Step 5: Ti layers and TiN layers are alternately plated on the titanium alloy substrate after bombardment and cleaning in step 4 by ion plating, wherein each Ti layer is composed of a plurality of Ti layer units, and the coating time of a single Ti layer unit is T Ti Each TiN layer consists of several TiN layer units, and the coating time of a single TiN layer unit is T TiN , and the plating time of each Ti layer and TiN layer is alternately nT in the direction from the cleaned titanium alloy substrate to the surface. Ti , 1T TiN , (n-1)T Ti , 2T TiN , ..., 1T Ti , nT TiN , n is a natural number greater than 3, and a transition layer is formed on the titanium alloy substrate; Step six: coating a TiN surface layer on the transition layer on the titanium alloy substrate in step five.
2. A transition layer design and preparation method based on the "slicing method" according to claim 1, characterized in that: The grinding and polishing process in step one is: the titanium alloy is grinded with sandpaper of #240, #400, #800, #1200, #1500, #2000 and #3000 in sequence, and then polished with diamond spray polishing agent with specifications of 0.5 μm and 0.1 μm respectively; the cleaning is carried out by ultrasonic treatment with anhydrous ethanol for 20 minutes.
3. A transition layer design and preparation method based on the "slicing method" according to claim 1, characterized in that: The mass purity of the Ti target in step 2 is above 99.99%; the mass purity of the argon and nitrogen in step 3 is above 99.99%, and the ion plating equipment is turned on and heated to 250°C, and the vacuum chamber is evacuated to 5×10 -3 Pa, and then filled with argon gas to a vacuum degree of 2×10 0 Pa, glow cleaning was performed for 15 min at a bias voltage of -1000 V, a duty cycle of 80%, and a temperature of 250°C.
4. The transition layer design and preparation method based on the "slicing method" according to claim 1 is characterized in that: In step 4, adjust the argon flow rate to a vacuum degree of 3×10 -1 Pa, bombardment cleaning was carried out for 5 min at a bombardment bias of -400 V, a bombardment current of 65 A, a duty cycle of 80%, and a temperature of 250°C.
5. The transition layer design and preparation method based on the "slicing method" according to claim 1 is characterized in that: The coating conditions of the single Ti layer unit in step 5 are: continuous argon gas flow, maintaining the working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150V, arc current to 60A, duty cycle to 80%, temperature to 250℃, coating time to T Ti The plating conditions of the single TiN layer unit are: maintaining the working vacuum degree of 3×10 -1 Pa, adjust the bias voltage to -150V, fill with nitrogen to a flow ratio of N2:Ar=7:1, arc current 60A, duty cycle 80%, temperature 250℃, coating time T TiN .
6. The transition layer design and preparation method based on the "slicing method" according to claim 1 is characterized in that: In step 5, the value of n is 3, 4, 5 or 6.
7. The transition layer design and preparation method based on the "slicing method" according to claim 1 is characterized in that: In step 5, from the (n+n 2 ) / 2 layer units later, the time length between each adjacent layer unit is (T Ti +T TiN ) / 2 interval, and then complete the subsequent plating in sequence.
8. The transition layer design and preparation method based on the "slicing method" according to claim 1 is characterized in that: The coating conditions for coating the TiN surface layer in step 6 are: maintaining a working vacuum of 3×10 -1 Pa, adjust the bias voltage to -150 V, arc current to 65 A, gas flow ratio N2:Ar = 7:1, temperature to 250 °C, and coating time to 40 min.