Preparation method of thin film HFS

By using high-temperature chemical vapor deposition method to form an α-Al2O3 film on the surface of nickel-based alloy, combined with ITO/In2O3 thermopile and Al2O3/YSZ thermal resistance layer, the problem of insulating attenuation of thin film heat flow sensor in high temperature environment is solved, and the insulating attenuation of thin film heat flow sensor in high temperature environment is achieved. Improved high temperature stability and measurement sensitivity.

CN118910564APending Publication Date: 2024-11-08LINGNAN NORMAL UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410843399.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The insulation attenuation of existing thin film heat flow sensors in high temperature environments leads to low measurement sensitivity and unstable, and the magnetron sputtering process limitations cannot provide sufficient electrical insulation.

Method used

The α-Al2O3 film was formed on the surface of the nickel-based alloy by high-temperature chemical vapor deposition, and combined with the ITO/In2O3 thermopile and the Al2O3/YSZ thermal resistance layer, the film HFS was prepared by magnetron sputtering and high-temperature welding technology, and 500℃ and 1000℃. Heat treatment is performed at °C to improve insulation and stability.

Benefits of technology

It improves the high-temperature insulation and stability of film HFS, enhances measurement sensitivity, avoids faults caused by thermal expansion mismatch, and maintains good electrical performance in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910564A_ABST
    Figure CN118910564A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a thin film HFS, which comprises the following steps: preparing a CVD-Al2O3 thin film structure on the surface of a nickel-based alloy by adopting an HTCVD (High Temperature Chemical Vapor Deposition) technology as a substrate: cleaning the substrate by using acetone, ethanol and deionized water to remove impurities and oil stains on the surface; an ITO / In2O3 thermopile is deposited on a cleaned CVD-Al2O3 substrate through the magnetron sputtering technology, a sensitive layer of the sensor is formed, ITO and In2O3 serve as p-type and n-type materials of the thermopile respectively, and thermocouple pairs arranged alternately are formed through a mask; aluminum oxide and YSZ materials are deposited at the cold end and the hot end of the sensitive layer through the magnetron sputtering technology, and a thermal resistance layer of the sensor is formed; on the outer side of the thermal resistance layer, a wire is connected with the cold end and the hot end of the thermopile through a high-temperature welding technology, and an output circuit of the thin film HFS is formed; the high-temperature insulativity and stability of the film layer are improved, and the prepared film HFS has good and stable performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high-temperature bearing heat flux density measurement, and in particular to a method for preparing a thin film HFS. Background Art

[0002] Bearings play an important role in the aerospace industry, such as aircraft engines and spacecraft propulsion systems. The performance and reliability of bearings directly affect the safety and life of aerospace equipment. Therefore, aerospace bearings need to undergo rigorous design, manufacturing, and testing. In these applications, the operating temperature of bearings has reached over 1000°C, far exceeding the melting point of bearing materials such as nickel-based alloys. In order to protect the bearings from being ablated by high-temperature airflow, high-temperature bearings need to be made into cooling channels to reduce the surface temperature and ensure that the bearings can operate normally when the hot airflow passes through. The indicator for evaluating the rationality of the cooling structure is the heat flux density. The heat flux density refers to the amount of heat passing through the bearing per unit time. By making a thin film heat flux sensor (HFS) on the surface of a high-temperature bearing, the heat flux density of the high-temperature bearing can be obtained, so as to further understand the heat conduction of the bearing in a high-temperature environment, and then optimize the design of the high-temperature bearing and improve the performance and life of the high-temperature bearing.

[0003] According to the boundary conditions of the heat conduction differential equation, there are two methods for measuring thin film HFS: 1) Devices based on the general assumption of semi-infinity, which calculate the heat flux by integrating the temperature over time, such as coaxial thermocouples and thin film resistor elements. However, devices based on the general assumption of semi-infinity need to be used when the heat flux changes rapidly, otherwise there will be problems with integral drift. The advantages of this device are simple structure and easy preparation process, but the disadvantages are low sensitivity, long response time, and inability to measure steady-state heat flux.

[0004] 2) Devices based on Fourier's law calculate heat flux according to the temperature gradient in the film thickness direction, have excellent dynamic and static performance, and are the main measurement method for thin film HFS. The sensitive structure of thin film HFS based on Fourier's law includes thermoelectric and thermal resistance, and is usually designed as a thermopile or bridge structure to increase sensitivity. This means that thin film HFS has a higher internal resistance than other thin film devices and requires higher electrical insulation in high temperature environments.

[0005] The preparation and performance of thin-film thermal flow sensors on the surface of nickel-based alloys are studied, among which the high-temperature insulation of the insulating layer is one of the key factors. There are three problems in the conventional magnetron sputtering preparation of aluminum oxide insulating layers: 1) In the magnetron sputtering process, the maximum preparation temperature of the aluminum oxide insulating layer cannot exceed 600°C. In order to convert the aluminum oxide crystal form into an α-phase structure, a long-term heat treatment of more than 1000°C is required. During this period, the main metal elements of the transition layer and the substrate diffuse into the aluminum oxide insulating layer to form NiFe compounds and Cr2O3. These substances have certain conductivity at high temperatures, resulting in a sharp attenuation of the high-temperature electrical insulation of the aluminum oxide film; 2) The volume shrinkage of the aluminum oxide crystal during the phase change destroys the adhesion of the alloy surface film; 3) Due to the limitation of the magnetron sputtering equipment, the aluminum oxide deposition thickness is too thin (1μm), which cannot provide sufficient electrical insulation under high temperature conditions. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a thin film HFS, which adopts a high-temperature chemical vapor deposition method to in-situ deposit and form an α-phase Al2O3 film on the surface of a nickel-based alloy, thereby improving the high-temperature insulation and stability of the film layer and ensuring that the prepared thin film HFS has good and stable performance.

[0007] In order to achieve the above objectives, the technical solution adopted by the present invention is: a method for preparing a thin film HFS, comprising the following steps: Step 1: Substrate preparation: Use HTCVD (high temperature chemical vapor deposition) technology to prepare a CVD-Al2O3 thin film structure on the surface of a nickel-based alloy as a substrate; Step 2, cleaning process: clean the CVD-Al2O3 substrate with acetone, ethanol and deionized water to remove impurities and oil stains on the surface; Step 3: Sputtering thermopile, ITO and In2O3: On the cleaned CVD-Al2O3 substrate, an ITO / In2O3 thermopile is deposited by magnetron sputtering technology to form the sensitive layer of the sensor. ITO and In2O3 are used as p-type and n-type materials of the thermopile, respectively, and an alternating arrangement of thermocouple pairs is formed through a mask. Step 4: Sputtering thermal resistance layer: Aluminum oxide and YSZ are deposited at the hot and cold ends of the sensitive layer by magnetron sputtering technology to form the thermal resistance layer of the sensor; Step 5: Wire welding: On the outside of the thermal resistance layer, connect the wires to the hot and cold ends of the thermopile through high-temperature welding technology to form the output circuit of the thin-film HFS.

[0008] Preferably, two multilayer films are deposited on the nickel alloy, namely a transition layer TiCN film and an insulating layer aluminum oxide film.

[0009] Preferably, in step 1, the average thickness of the aluminum oxide layer is about 7 μm.

[0010] Preferably, in step three, the average thickness of the sputtered ITO film is 1 μm, and the average thickness of the sputtered In2O3 film is 1 μm.

[0011] Preferably, the average thickness of the Al2O3 / YSZ film sputtered in step 4 is 0.4 μm.

[0012] Preferably, the HFS film prepared in step 5 is heat treated at 500° C. for 4 hours in a nitrogen environment.

[0013] Preferably, after the heat treatment in the nitrogen environment is completed, heat treatment is performed at 1000° C. for 1 hour in an air environment to form a thermally grown oxide layer.

[0014] Preferably, the heat treatment device used for heat treatment includes a heat treatment box, which is equipped with a sealing cover and has a nitrogen charging and discharging interface and an air charging and discharging interface installed on the side. A heat treatment frame is arranged in the heat treatment box, a supporting placement plate is installed in the middle of the heat treatment frame, a heat source is installed at the lower part of the heat treatment frame, and the heights of the nitrogen charging and discharging interface and the inflation charging and discharging interface are lower than the upper end of the heat treatment frame.

[0015] The technical effects of the present invention are: α-Al2O3 thin film is prepared in situ by high temperature chemical vapor deposition (HTCVD) to improve high temperature resistance; then thin film sensor is made on the α-Al2O3 thin film to measure heat flux density. The transparent conductive oxide thermopile composed of ITO and In2O3 has good high temperature stability and high thermoelectric potential output, which can replace precious metals. The thermal expansion coefficient (CTE) of ITO / In2O3 is 7~8×10 -6 / K, close to Al2O3 film (CTE 8~8.2×10 -6 / K), so it can avoid failures caused by thermal mismatch in high temperature environments and is the best choice for thin film HFS; the application of CVD-Al2O3 helps to improve the stability of thin film HFS. The sensitivity of thin film HFS based on 7μm CVD-Al2O3 is close to that of thin film HFS based on 100μm thermal sprayed Al2O3.

[0016] Al2O3 / YSZ film is used as the thermal resistance layer to increase the temperature difference between the hot and cold ends and improve the sensitivity of the sensor.

[0017] The heat flux sensor was heat treated at 500°C for 4 hours to improve the crystallinity and stability of the film; then it was heat treated at 1000°C for 1 hour in an air environment to form a thermally grown oxide layer and improve the insulation of the film.

[0018] 4. The heat treatment device can avoid the airflow generated during the process of filling and discharging nitrogen or air from affecting the thin film HFS through the design of the heat treatment frame. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the microstructure diagram of CVD-Al2O3 film.

[0020] Figure 2 This is the XRD analysis diagram of CVD-Al2O3 film.

[0021] Figure 3 This is the HFS morphology of the film.

[0022] Figure 4 Schematic diagram of the heat treatment device.

[0023] Figure 5 This is a graph showing the test results of the intrinsic high-temperature insulation properties of the film layer of Example 3.

[0024] Figure 6 This is the test result of intrinsic high temperature insulation of NiCrAlY-TGO-Al2O3 film.

[0025] The text labels shown in the figure indicate: 1. heat treatment box; 2. sealing cover; 3. nitrogen charging and discharging interface; 4. air charging and discharging interface; 5. heat treatment frame; 6. support placement plate; 7. temperature sensor. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings. The description in this part is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention. Example 1

[0027] The method for preparing the HFS thin film comprises the following steps: Step 1: Substrate preparation: Use HTCVD (high temperature chemical vapor deposition) technology to prepare a CVD-Al2O3 thin film structure on the surface of a nickel-based alloy as a substrate; Step 2, cleaning process: clean the CVD-Al2O3 substrate with acetone, ethanol and deionized water to remove impurities and oil stains on the surface; Step 3: Sputtering thermopile, ITO and In2O3: On the cleaned CVD-Al2O3 substrate, an ITO / In2O3 thermopile is deposited by magnetron sputtering technology to form the sensitive layer of the sensor. ITO and In2O3 are used as p-type and n-type materials of the thermopile, respectively, and an alternating arrangement of thermocouple pairs is formed through a mask. Step 4: Sputtering thermal resistance layer: Aluminum oxide and YSZ are deposited at the hot and cold ends of the sensitive layer by magnetron sputtering technology to form the thermal resistance layer of the sensor; Step 5: Wire welding: On the outside of the thermal resistance layer, connect the wires to the hot and cold ends of the thermopile through high-temperature welding technology to form the output circuit of the thin-film HFS. Example 2

[0028] The method for preparing the HFS thin film comprises the following steps: Step 1: Substrate preparation: Two multilayer films, namely, transition layer TiCN film and insulating layer aluminum oxide film, are deposited on nickel alloy using HTCVD (high temperature chemical vapor deposition) technology as the substrate; the average thickness of the aluminum oxide layer is about 7μm.

[0029] Step 2, cleaning process: clean the CVD-Al2O3 substrate with acetone, ethanol and deionized water to remove impurities and oil stains on the surface; Step 3: Sputtering thermopile, ITO and In2O3: On the cleaned CVD-Al2O3 substrate, an ITO / In2O3 thermopile is deposited by magnetron sputtering technology to form the sensitive layer of the sensor. ITO and In2O3 are used as p-type and n-type materials of the thermopile respectively, and an alternating arrangement of thermocouple pairs is formed through a mask; the average thickness of the ITO film is 1μm, and the average thickness of the sputtered In2O3 film is 1μm; Step 4: Sputtering thermal resistance layer: Aluminum oxide and YSZ are deposited at the hot and cold ends of the sensitive layer by magnetron sputtering technology to form the thermal resistance layer of the sensor. The average thickness of the Al2O3 / YSZ film is 0.4μm. Step 5: Wire welding: On the outside of the thermal resistance layer, connect the wires to the hot and cold ends of the thermopile through high-temperature welding technology to form the output circuit of the thin-film HFS. Example 3

[0030] The method for preparing the HFS thin film comprises the following steps: Step 1: Substrate preparation: Two multilayer films, namely, transition layer TiCN film and insulating layer aluminum oxide film, are deposited on nickel alloy using HTCVD (high temperature chemical vapor deposition) technology as the substrate; the average thickness of the aluminum oxide layer is about 7μm.

[0031] Step 2, cleaning process: clean the CVD-Al2O3 substrate with acetone, ethanol and deionized water to remove impurities and oil stains on the surface; Step 3: Sputtering thermopile, ITO and In2O3: On the cleaned CVD-Al2O3 substrate, an ITO / In2O3 thermopile is deposited by magnetron sputtering technology to form the sensitive layer of the sensor. ITO and In2O3 are used as p-type and n-type materials of the thermopile respectively, and an alternating arrangement of thermocouple pairs is formed through a mask; the average thickness of the ITO film is 1μm, and the average thickness of the sputtered In2O3 film is 1μm; Step 4: Sputtering thermal resistance layer: Aluminum oxide and YSZ are deposited at the hot and cold ends of the sensitive layer by magnetron sputtering technology to form the thermal resistance layer of the sensor. The average thickness of the Al2O3 / YSZ film is 0.4μm. Step 5, wire welding: On the outside of the thermal resistance layer, connect the wires to the hot and cold ends of the thermopile through high-temperature welding technology to form the output circuit of the thin film HFS; Step 6: Perform heat treatment at 500° C. for 4 h in a nitrogen environment, and then perform heat treatment at 1000° C. for 1 h in an air environment to form a thermally grown oxide layer.

[0032] The heat treatment device used is as follows Figure 4 As shown, it includes a heat treatment box 1, the heat treatment box 1 is equipped with a sealing cover 2, and a nitrogen charging and discharging interface 3 and an air charging and discharging interface 4 are installed on the side, a heat treatment frame 5 is arranged in the heat treatment box 1, a supporting placement plate 6 is installed in the middle of the heat treatment frame 5, a heat source is installed at the lower part of the heat treatment frame 5, and the heights of the nitrogen charging and discharging interface 3 and the air charging and discharging interface 4 are lower than the upper end of the heat treatment frame 5.

[0033] The heat treatment operation of step six is ​​performed by the above-mentioned heat treatment device as follows: first open the sealing cover 2, then place the film HFS on the supporting placement plate 6, then cover the sealing cover 2, and then fill it into the heat treatment box through the nitrogen charging and discharging device connected to the nitrogen charging and discharging interface 3. When the gas is charged and discharged, an airflow will be formed. The present application uses the design of the heat treatment frame 5 to block the airflow to prevent the airflow from affecting the placed film HFS; after the nitrogen is filled, the heat source is controlled to generate heat so that the temperature sensed by the temperature sensor is 500°C, and the heat preservation treatment is performed for 4 hours, and then the nitrogen is extracted, and air is filled in through the air charging and discharging device connected to the air charging and discharging interface 4, and the heat source is controlled to generate heat so that the temperature sensed by the temperature sensor is 1000°C, and it is maintained for 1 hour, and the heat treatment of step six is ​​completed.

[0034] The aluminum oxide film obtained in step 1 of this embodiment 3 is as follows Figure 1 and Figure 2 As shown, the film surface is dense and the crystal structure of the film is mainly composed of α-Al2O3.

[0035] The aluminum oxide insulating layer was prepared by plasma thermal spraying (PST) and physical vapor deposition (PVD) processes; and a thin film HFS was prepared thereon. It was used to evaluate the performance and advantages of the CVD-Al2O3 thin film HFS of Example 3. The plasma thermal spraying (PST) process is to heat the aluminum oxide powder and spray it onto the alloy surface using a plasma flame to form an aluminum oxide coating with a thickness of about 100μm. The physical vapor deposition (PVD) process is to sputter the aluminum oxide target material onto the alloy surface using magnetron sputtering to form an aluminum oxide film with a thickness of about 1μm.

[0036] In order to evaluate the effect of CVD-Al2O3 insulation layer at high temperature, the longitudinal insulation resistance of the aluminum oxide film was obtained according to the change of temperature, such as Figure 5 As shown in the figure, the sample was repeatedly heated at 850℃ for 9 cycles. The experimental results show that when the test temperature is less than 600℃, the insulation resistance exceeds the test range of the data collector, so no accurate value is obtained. When the temperature is increased from 600℃ to 750℃, the insulation resistance drops sharply from 120 MΩ to 20 MΩ. At 830℃, the insulation resistance slowly drops from 20 MΩ to 10 MΩ. It can be seen that the aluminum oxide insulation layer prepared by HTCVD has good electrical insulation properties at high temperatures, which ensures the stability of the thin film HFS film on the nickel alloy.

[0037] Compare the insulation effects of films prepared by physical vapor deposition (PVD) processes, such as Figure 6 The longitudinal resistance of the NiCrAlY-TGO-Al2O3 film layer shown in the figure decreases with increasing temperature, but still remains at a high level, indicating that the film layer prepared by the physical vapor deposition (PVD) process has good high-temperature insulation properties; however, the longitudinal resistance of the film layer is affected by the oxidation and loosening of the metal pad in a high temperature environment, resulting in fluctuations in the resistance value and the appearance of breakpoints, indicating that the stability and reliability of the PVD-Al2O3 film need to be further improved.

[0038] The insulation effect of the film layer prepared by plasma thermal spraying (PST) process. The Al2O3 insulation layer with a thickness of 100μm was prepared by plasma spraying process to improve the high-temperature insulation performance of the thin film heat flow sensor on the surface of nickel-based alloy.

[0039] The sensitivity of the 7 μm CVD-Al 2 O 3 thin film HFS obtained in Example 3 of the present application is close to that of the 100 μm thermal sprayed Al 2 O 3 thin film HFS.

[0040] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0041] This article uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. The above is only a preferred implementation of the present invention. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, ordinary technicians in this technical field can make several improvements, modifications or changes without departing from the principles of the present invention, and can also combine the above technical features in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the inventive concept and technical solution to other occasions without improvement, should be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a thin film HFS, characterized in that: The steps include: Step 1: Substrate preparation: Use HTCVD (high temperature chemical vapor deposition) technology to prepare a CVD-Al2O3 thin film structure on the surface of a nickel-based alloy as a substrate; Step 2, cleaning process: clean the CVD-Al2O3 substrate with acetone, ethanol and deionized water to remove impurities and oil stains on the surface; Step 3: Sputtering thermopile, ITO and In2O3: On the cleaned CVD-Al2O3 substrate, an ITO / In2O3 thermopile is deposited by magnetron sputtering technology to form the sensitive layer of the sensor. ITO and In2O3 are used as p-type and n-type materials of the thermopile, respectively, and an alternating arrangement of thermocouple pairs is formed through a mask. Step 4: Sputtering thermal resistance layer: Aluminum oxide and YSZ are deposited at the hot and cold ends of the sensitive layer by magnetron sputtering technology to form the thermal resistance layer of the sensor; Step 5: Wire welding: On the outside of the thermal resistance layer, connect the wires to the hot and cold ends of the thermopile through high-temperature welding technology to form the output circuit of the thin-film HFS.

2. The method for preparing the thin film HFS according to claim 1, characterized in that: In step 1, two multilayer films are deposited on the nickel alloy, namely a transition layer TiCN film and an insulating layer aluminum oxide film.

3. The method for preparing the thin film HFS according to claim 1 or 2, characterized in that: The average thickness of the aluminum oxide layer in step 1 is 7 μm.

4. The method for preparing the thin film HFS according to claim 1, characterized in that: In step 3, the average thickness of the sputtered ITO film is 1 μm, and the average thickness of the sputtered In2O3 film is 1 μm.

5. The method for preparing the HFS thin film according to claim 1, characterized in that: The average thickness of the sputtered Al2O3 / YSZ film in step 4 is 0.4 μm.

6. The method for preparing the thin film HFS according to claim 1, characterized in that: The HFS film prepared in step 5 was heat treated at 500° C. for 4 h in a nitrogen environment.

7. The method for preparing the thin film HFS according to claim 6, characterized in that: After the nitrogen environment heat treatment is completed, heat treatment is performed at 1000° C. for 1 hour in an air environment to form a thermally grown oxide layer.

8. The method for preparing the thin film HFS according to claim 7, characterized in that: The heat treatment device used for heat treatment includes a heat treatment box, which is equipped with a sealing cover and has a nitrogen charging and discharging interface and an air charging and discharging interface installed on the side. A heat treatment frame is arranged in the heat treatment box, a supporting placement plate is installed in the middle of the heat treatment frame, a heat source is installed at the lower part of the heat treatment frame, and the heights of the nitrogen charging and discharging interface and the air charging and discharging interface are lower than the upper end of the heat treatment frame.

Citation Information

Cited By

  • Miniature transient film heat flow sensor

    CN121855713A

  • A miniature transient thin-film heat flux sensor