NiFe-LDH loaded PbO2 composite catalyst, preparation method thereof and application of NiFe-LDH loaded PbO2 composite catalyst in seawater oxidation catalysis

By depositing PbO2 nanoparticles on the surface of the NiFe-LDH catalyst to form a dense film, the problem of insufficient corrosion resistance of NiFe-LDH catalyst in seawater electrolysis is solved, and efficient redox catalytic performance and stability improvement in seawater is achieved.

CN118910658APending Publication Date: 2024-11-08QINGDAO UNIV OF SCI & TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410931621.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing NiFe-LDH catalysts have problems with insufficient corrosion resistance in seawater electrolysis, especially at high anode current or potential, which leads to a reduction in catalyst structure loss and OER selectivity.

Method used

NiFe-LDH was synthesized on the foam nickel support by solvothermal method, and a dense film composed of PbO2 nanoparticles was formed on its surface by constant current deposition to form a NiFe-LDH@PbO2 composite structure to improve the conductivity and mass transfer rate of the catalyst. and stability, inhibiting the migration of chloride ions.

Benefits of technology

It significantly improves the catalyst's anti-chlorine ion corrosion ability and OER selectivity, extends the service life of the catalyst, maintains excellent catalytic performance in alkaline seawater, and has good corrosion resistance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910658A_ABST
    Figure CN118910658A_ABST
Patent Text Reader

Abstract

The invention discloses a NiFe-LDH loaded PbO2 composite catalyst as well as a preparation method and application thereof in catalysis of seawater oxidation. The preparation method specifically comprises the following steps: firstly, synthesizing NiFe-LDH on foamed nickel by adopting a hydrothermal method, and then electrically depositing a layer of compact film consisting of PbO2 nanoparticles on the surface of a NiFe-LDH nanosheet, so as to prepare the NiFe-LDH-coated PbO2 composite catalyst. The existence of the PbO2 dense membrane can selectively inhibit chloride ions from entering the surface of the catalyst, so that the chloride ion corrosion resistance and seawater oxidation selectivity of the catalyst are greatly improved; and the PbO2 film layer can also prevent the catalyst from leaking, so that the stability of the catalyst in catalytic oxidation of alkaline seawater is improved. Therefore, the NiFe-LDH-coated PbO2 electrode shows excellent oxygen evolution catalytic selectivity and stability in alkaline simulated seawater and alkaline natural seawater electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention belongs to the field of new energy material technology and electrochemical catalysis, and specifically relates to a NiFe-LDH loaded PbO2 composite catalyst; it also relates to a preparation method of the catalyst and its application in electrocatalytic seawater anode oxygen evolution reaction. Background technology:

[0002] Seawater electrolysis produces high-calorie hydrogen (142MJ kg -1 ) is becoming increasingly attractive in the field of renewable energy conversion and storage. Electrochemical seawater splitting can effectively utilize renewable electricity from intermittent clean wind, nuclear and solar power, which is more abundant in arid desert areas near the coast. More importantly, the nearly unlimited seawater raw material (~97% of total water resources) can save scarce fresh water and even reversely produce pure water for coastal areas with insufficient fresh water. However, due to the presence of chloride ions (~0.5M) and other complex components, the realization of seawater electrolysis is more challenging than freshwater electrolysis. One of the biggest challenges of seawater electrolysis is Cl - The chlorine evolution reaction (CER) in which chlorine is oxidized to form Cl2 in acidic electrolytes and the hypochlorite oxidation reaction (HCER) in which chlorine is oxidized to form hypochlorite in alkaline media will both compete with OER in the reaction process.

[0003] In view of the above basic principles, alkaline electrolytes are usually used to enhance the selectivity of OER. - An effective solution to the corrosion problem is to develop catalyst electrodes with high activity and high corrosion resistance. Recently, nickel-iron layered double hydroxide (NiFe-LDH) has been demonstrated to be the most advanced alkaline water oxidation catalyst due to its unique layered structure and inherent electrocatalytic activity. However, its poor corrosion resistance has largely hindered its further application in seawater electrolysis. Therefore, in order to improve the corrosion stability of NiFe-LDH-based electrodes, a variety of protective measures have been taken. For example, transition metal sulfides, phosphides, borides, selenides, etc. can be electrochemically oxidized in situ to form a passivation film of sulfate, phosphate, borate or selenate, which electrostatically repels Cl - Anions are used to improve the corrosion resistance of the catalyst. However, these oxygen anions are continuously leached from the catalyst into the electrolyte at high anode current or potential. After repeated electrolyte renewal, excessive loss of oxygen-containing anions will destroy the structure of the catalyst. It is reported that MnO x 、CeO x Cr y O xTransition metal oxide layers can selectively prevent chloride ions from entering the catalyst surface, thereby improving the catalyst's resistance to chloride ion corrosion. Lead oxide does not have OER catalytic performance, but it has certain potential in inhibiting chloride ion corrosion as an oxide layer. Considering that three-dimensional heterostructured catalysts can provide a large surface area and abundant active sites in the electrolysis of seawater, there has been no report on the construction of a heterostructure of NiFe-LDH and lead oxide nanoparticles composites and their use as seawater OER electrocatalysts.

[0004] The present invention utilizes a solvothermal method to synthesize NiFe-LDH on a nickel foam (NF) carrier, and under optimal electrodeposition conditions, a dense film composed of PbO2 nanoparticles is electrodeposited on the surface of the NiFe-LDH nanosheet to obtain a NiFe-LDH@PbO2 nanocomposite structure, thereby improving the conductivity, mass transfer rate and stability of the catalyst. Since the PbO2 nanoparticles form a dense film, the migration of chloride ions can be selectively inhibited, the catalyst's resistance to chloride ion corrosion is improved, and thus the OER selectivity is improved; the PbO2 film layer can also prevent catalyst leakage, thereby improving the catalyst's OER stability in alkaline seawater. Therefore, the NiFe-LDH@PbO2 electrode shows excellent OER catalytic performance in both alkaline simulated seawater and alkaline natural seawater electrolytes. The invention has important theoretical and practical significance for the development of stability repair of transition metal-based anode catalysts in electrolyzed seawater and energy conversion and storage devices. Summary of the invention:

[0005] In view of the deficiencies in the prior art and the needs of research and application in this field, one of the purposes of the present invention is to provide a NiFe-LDH-loaded PbO2 composite catalyst, characterized in that the catalyst is a composite structure formed by depositing a dense film composed of PbO2 nanoparticles on a NiFe-LDH sheet; the PbO2 nanofilm in the catalyst is prepared by constant current deposition technology under the conditions of optimal deposition time, current density and supporting electrolyte concentration; the catalyst is in-situ grown on nickel foam, denoted as NiFe-LDH@PbO2;

[0006] The second object of the present invention is to provide a method for preparing a NiFe-LDH-loaded PbO2 composite catalyst, comprising the following specific steps:

[0007] (a) Preparation of NiFe-LDH

[0008] The size is 2×3cm 2The sheet-like nickel foam was placed in 3M HCl, deionized water, and anhydrous ethanol in turn, and ultrasonically treated for 15 minutes each, rinsed with deionized water for several times, and dried in an oven at 50°C; 1mmol of Ni(NO3)2·6H2O, 0.5mmol of Fe(NO3)3·9H2O, and 5mmol of urea were dissolved in 30mL of deionized water, and the mixed solution and the treated nickel foam were transferred to an 80mL polytetrafluoroethylene autoclave, reacted at 120°C for 12 hours, and the nickel foam was taken out after cooling to room temperature, and washed with ultrapure water and ethanol for several times, respectively, and dried naturally at 50°C to obtain NiFe-LDH;

[0009] (b) Preparation of NiFe-LDH@PbO2

[0010] The NiFe-LDH prepared in step (a) was cut into 1×2 cm 2 specifications, using it as the working electrode, Pt wire as the counter electrode, and Ag / AgCl electrode as the reference electrode. The concentration is 100 mmol L -1 The concentration of NaNO3 is 5~200mmol L -1 The Pb(NO3)2 mixed solution is used as the electrolyte, and the current density is 5-30mA -2 , a constant current deposition is performed under the condition of a deposition time of 60 to 1800 s to grow a PbO2 film on its surface. After the deposition is completed, the working electrode is removed and rinsed with deionized water, and then dried in an oven at 50°C to obtain an electrocatalyst NiFe-LDH@PbO2;

[0011] In the NiFe-LDH loaded PbO2 composite catalyst, PbO2 is covered on the surface of NiFe-LDH nanosheets in the form of a film formed by connecting nanoparticles. The particle size of the PbO2 nanoparticles is less than 5nm and the thickness is less than 3nm. The lateral size of the NiFe-LDH nanosheets is 200-350nm and the thickness is 20-30nm.

[0012] The third object of the present invention is to provide a NiFe-LDH loaded PbO2 composite catalyst for electrocatalytic application in the alkaline seawater oxidation process; specifically, the catalyst NiFe-LDH@PbO2 is 1 mol L -1 KOH and 2.5 mol L -1 In the aqueous solution of NaCl, the dense nanofilm formed by PbO2 nanoparticles covering the surface of NiFe-LDH nanosheets can selectively inhibit the entry of chloride ions into the surface of NiFe-LDH nanosheets. -2After 150 hours of chronopotentiometry under a current density of , the catalytic performance showed little attenuation, and the catalyst structure and substrate framework remained basically intact. However, NiFe-LDH broke after only 2 hours of chronopotentiometry under the same conditions.

[0013] Compared with the prior art, the present invention has the following main advantages and beneficial effects:

[0014] 1) The NiFe-LDH loaded PbO2 composite catalyst of the present invention is a non-precious metal material, the raw materials used are easy to purchase, the resources are abundant and the cost is low, the experimental method is easy to operate, and it is convenient for large-scale production;

[0015] 2) The NiFe-LDH loaded PbO2 composite catalyst described in the present invention has good OER catalytic selectivity, corrosion resistance and stability in chloride ion-containing electrolytes, and has obvious advantages over precious metal catalysts. Description of the drawings:

[0016] Figure 1 They are scanning electron microscope images of NiFe-LDH obtained in Comparative Example 1 (left) and NiFe-LDH@PbO2 obtained in Example 1 (right).

[0017] Figure 2 XRD diagrams of NiFe-LDH obtained in Comparative Example 1 and NiFe-LDH@PbO2 obtained in Example 1.

[0018] Figure 3 NiFe-LDH@PbO2 obtained in Example 1 and NiFe-LDH@PbO2-5, NiFe-LDH@PbO2-20, NiFe-LDH@PbO2-100 and NiFe-LDH@PbO2-200 obtained in Example 2 were prepared at 1 mol L -1 KOH + 0.5 mol L -1 LSV curves of OER in NaCl medium.

[0019] Figure 4 The NiFe-LDH@PbO2 obtained in Example 1 and the NiFe-LDH@PbO2-60s, NiFe-LDH@PbO2-300s, NiFe-LDH@PbO2-600s and NiFe-LDH@PbO2-1200s obtained in Example 3 were prepared in 1 mol L -1 KOH + 0.5 mol L -1 LSV curves of OER in NaCl medium.

[0020] Figure 5NiFe-LDH@PbO2 obtained in Example 1 and NiFe-LDH@PbO2-5m, NiFe-LDH@PbO2-20m and NiFe-LDH@PbO2-30m obtained in Example 4 were prepared in 1 mol L -1 KOH + 0.5 mol L -1 LSV curves of OER in NaCl medium.

[0021] Figure 6 NiFe-LDH obtained in Comparative Example 1 and NiFe-LDH@PbO2 obtained in Example 1 were prepared in 1 mol L -1 KOH + 0.5 mol L -1 LSV curves of OER in NaCl medium.

[0022] Figure 7 NiFe-LDH obtained in Comparative Example 1 and NiFe-LDH@PbO2 obtained in Example 1 were heated to 1.0 mol L -1 KOH + 2.5 mol L -1 In NaCl medium, 250 mA cm -2 Chronopotentiometry curves at current density of 2.5 and optical photographs of the corresponding electrodes after stabilization.

[0023] Figure 8 Example 1 NiFe-LDH@PbO2 obtained in 1.0 mol L -1 KOH + 2.5 mol L -1 In NaCl medium, 250 mA cm -2 LSV curves before and after 150 hours of chronopotentiometry.

[0024] Fig. 9 The NiFe-LDH obtained in Comparative Example 1 and the NiFe-LDH@PbO2 obtained in Example 1 were respectively - 1 KOH + 0.5 mol L -1 NaCl (left) and 1.0 mol L -1 Comparison of the corrosion polarization curves in KOH+natural seawater (right) and the bar graphs of the corresponding corrosion potentials and corrosion currents. Specific implementation method:

[0025] For a further understanding of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited in any way.

[0026] Embodiment 1:

[0027] (a) Preparation of NiFe-LDH

[0028] The size is 2×3cm 2 The sheet-like nickel foam was placed in 3M HCl, deionized water, and anhydrous ethanol in turn, and ultrasonically treated for 15 minutes each, rinsed with deionized water for several times, and dried in an oven at 50°C; 1mmol of Ni(NO3)2·6H2O, 0.5mmol of Fe(NO3)3·9H2O, and 5mmol of urea were dissolved in 30mL of deionized water, and the mixed solution and the treated nickel foam were transferred to an 80mL polytetrafluoroethylene autoclave, reacted at 120°C for 12 hours, and the nickel foam was taken out after cooling to room temperature, and washed with ultrapure water and ethanol for several times, respectively, and dried naturally at 50°C to obtain NiFe-LDH;

[0029] (b) Preparation of NiFe-LDH@PbO2

[0030] The NiFe-LDH prepared in step (a) was cut into 1×2 cm 2 specifications, using it as the working electrode, Pt wire as the counter electrode, and Ag / AgCl electrode as the reference electrode. The concentration is 100 mmol L -1 The concentration of NaNO3 is 10 mmol L -1 The Pb(NO3)2 mixed solution was used as electrolyte and the current density was 10 mA. -2 , constant current deposition was performed under the condition of deposition time of 120s to grow PbO2 film on its surface. After the deposition was completed, the working electrode was removed and rinsed with deionized water, and dried in an oven at 50°C to obtain the electrocatalyst NiFe-LDH@PbO2;

[0031] Embodiment 2:

[0032] (a) Preparation of NiFe-LDH

[0033] Prepared according to the method and conditions of step (a) in Example 1;

[0034] (b) Preparation of NiFe-LDH@PbO2

[0035] The NiFe-LDH prepared in step (a) was cut into 1×2 cm 2 specifications, using it as the working electrode, Pt wire as the counter electrode, and Ag / AgCl electrode as the reference electrode. The concentration is 100 mmol L -1 The concentrations of NaNO3 were 5, 20, 100, and 200 mmol L -1 The Pb(NO3)2 mixed solution was used as electrolyte and the current density was 10 mA. -2, constant current deposition was performed under the condition of a deposition time of 120 s to grow a PbO2 film on its surface. After the deposition was completed, the working electrode was removed and rinsed with deionized water, and dried in an oven at 50°C to obtain electrocatalysts NiFe-LDH@PbO2-5, NiFe-LDH@PbO2-20, NiFe-LDH@PbO2-100 and NiFe-LDH@PbO2-200;

[0036] Embodiment 3:

[0037] (a) Preparation of NiFe-LDH

[0038] Prepared according to the method and conditions of step (a) in Example 1;

[0039] (b) Preparation of NiFe-LDH@PbO2

[0040] The NiFe-LDH prepared in step (a) was cut into 1×2 cm 2 specifications, using it as the working electrode, Pt wire as the counter electrode, and Ag / AgCl electrode as the reference electrode. The concentration is 100 mmol L -1 The concentration of NaNO3 is 10 mmol L -1 The Pb(NO3)2 mixed solution was used as electrolyte and the current density was 10 mA. -2 , constant current deposition was carried out under the conditions of deposition time of 60, 300, 600 and 1200 s respectively, so that PbO2 film grew on its surface. After the deposition was completed, the working electrode was removed and rinsed with deionized water, and dried in an oven at 50°C to obtain electrocatalysts NiFe-LDH@PbO2-60s, NiFe-LDH@PbO2-300s, NiFe-LDH@PbO2-600s and NiFe-LDH@PbO2-1200s;

[0041] Embodiment 4:

[0042] (a) Preparation of NiFe-LDH

[0043] Prepared according to the method and conditions of step (a) in Example 1;

[0044] (b) Preparation of NiFe-LDH@PbO2

[0045] The NiFe-LDH prepared in step (a) was cut into 1×2 cm 2 specifications, using it as the working electrode, Pt wire as the counter electrode, and Ag / AgCl electrode as the reference electrode. The concentration is 100 mmol L -1 The concentration of NaNO3 is 10 mmol L -1The Pb(NO3)2 mixed solution was used as the electrolyte at current densities of 5, 20, and 30 mA cm -2 , constant current deposition was performed under the condition of a deposition time of 120 s to grow a PbO2 film on its surface. After the deposition was completed, the working electrode was removed and rinsed with deionized water, and then dried in an oven at 50°C to obtain electrocatalysts NiFe-LDH@PbO2-5m, NiFe-LDH@PbO2-20m and NiFe-LDH@PbO2-30m;

[0046] Comparative Example 1:

[0047] Preparation of NiFe-LDH

[0048] Prepared according to the method and conditions of step (a) in Example 1;

[0049] Figure 1 The scanning electron microscope images of NiFe-LDH obtained in Comparative Example 1 (left) and NiFe-LDH@PbO2 obtained in Example 1 (right) are shown respectively. As shown in the left figure, the SEM image shows typical quasi-hexagonal LDH nanosheets with smooth surfaces. The lateral dimensions of these nanosheets are about 200-350nm and the thickness is about 15-20nm. NiFe-LDH nanosheets grow vertically on the NF substrate and are interlaced with each other, presenting a layered 3D structure. After the PbO2 layer is introduced by electrodeposition, the morphology of the LDH nanosheets does not change, but it can be clearly seen that the surface of the NiFe-LDH nanosheet is covered with a dense film formed by connecting nanoparticles, the thickness of which is less than 3nm. Although the lateral dimensions of the NiFe-LDH@PbO2 nanosheets remain unchanged, due to the coverage of the PbO2 nanofilm, its thickness increases to 20-30nm, see the right figure. The presence of the PbO2 nanofilm can selectively inhibit the entry of chloride ions into the surface of the NiFe-LDH nanosheets, thereby improving the OER selectivity, corrosion resistance and stability of the catalyst in the seawater medium.

[0050] Figure 2 The XRD patterns of NiFe-LDH obtained in Comparative Example 1 and NiFe-LDH@PbO2 obtained in Example 1 are shown in the figure. It can be seen from the figure that both samples have very strong diffraction peaks of the nickel foam substrate. In addition, both samples show weak characteristic diffraction peaks of NiFe-LDH. However, compared with NiFe-LDH, NiFe-LDH@PbO2 has additional diffraction peaks of the (200) and (211) crystal planes of PbO2 at 36.2° and 50.1°, which proves that PbO2 is deposited on the surface of NiFe-LDH nanosheets.

[0051] The following electrocatalytic performance tests all used a saturated Hg / HgO electrode as the reference electrode, a graphite rod electrode as the counter electrode, and a scan rate of 5 mV / s.

[0052] Figure 3 NiFe-LDH@PbO2 obtained in Example 1 and NiFe-LDH@PbO2-5, NiFe-LDH@PbO2-20, NiFe-LDH@PbO2-100 and NiFe-LDH@PbO2-200 obtained in Example 2 were prepared at 1 mol L -1 KOH + 0.5 mol L -1 LSV curve of OER in NaCl medium. It can be seen from the figure that when the concentration of Pb(NO3)2 in the electrolyte is 10mmol L -1 The OER performance of the catalyst in alkaline simulated seawater is optimal.

[0053] Figure 4 The NiFe-LDH@PbO2 obtained in Example 1 and the NiFe-LDH@PbO2-60s, NiFe-LDH@PbO2-300s, NiFe-LDH@PbO2-600s and NiFe-LDH@PbO2-1200s obtained in Example 3 were prepared in 1 mol L -1 KOH + 0.5 mol L -1 LSV curve of OER in NaCl medium. It can be seen from the figure that when PbO2 is electrodeposited, the OER performance of the catalyst in alkaline simulated seawater is optimal when the deposition time is 120s.

[0054] Figure 5 NiFe-LDH@PbO2 obtained in Example 1 and NiFe-LDH@PbO2-5m, NiFe-LDH@PbO2-20m and NiFe-LDH@PbO2-30m obtained in Example 4 were prepared in 1 mol L -1 KOH + 0.5 mol L -1 LSV curve of OER in NaCl medium. It can be seen from the figure that when PbO2 is deposited at constant potential, the deposition current density is 10mAcm -2 The OER performance of the catalyst in alkaline simulated seawater is optimal.

[0055] Figure 6 NiFe-LDH obtained in Comparative Example 1 and NiFe-LDH@PbO2 obtained in Example 1 were prepared in 1 mol L -1 KOH + 0.5 mol L -1 LSV curve of OER in NaCl medium. As can be seen from the figure, the OER performance of NiFe-LDH@PbO2 prepared under the optimal deposition conditions in alkaline simulated seawater is basically close to that of NiFe-LDH, so the following mainly discusses the corrosion resistance and stability of the two catalysts in alkaline seawater medium.

[0056] Figure 7 NiFe-LDH obtained in Comparative Example 1 and NiFe-LDH@PbO2 obtained in Example 1 were heated to 1.0 mol L -1 KOH + 2.5 mol L -1 In NaCl medium, 250 mA cm -2 The chronoamperometric curves and the optical photographs of the corresponding electrodes after stabilization show that NiFe-LDH@PbO2 can -2 After 150 hours of chronopotentiometry at a current density of 1.50, the catalytic performance did not decay, and the catalyst structure and substrate framework remained intact. However, NiFe-LDH broke after only 2 hours of chronopotentiometry under the same conditions. This is mainly due to the dense PbO2 nanofilm formed on the surface of NiFe-LDH nanosheets, which can selectively inhibit chloride ions from entering the surface of NiFe-LDH nanosheets, thereby greatly improving the corrosion resistance and stability of NiFe-LDH@PbO2 catalysts in alkaline simulated seawater.

[0057] Figure 8 Example 1 NiFe-LDH@PbO2 obtained in 1.0 mol L -1 KOH + 2.5 mol L -1 In NaCl medium, 250 mA cm -2 LSV curves before and after 150 hours of chronopotentiometry. As can be seen from the figure, the LSV curves before and after 150 hours are not much different, especially at a current density of 400 mA cm -2 The two curves are close to intersecting, indicating that NiFe-LDH@PbO2 has good stability at high current density.

[0058] Fig. 9 The NiFe-LDH obtained in Comparative Example 1 and the NiFe-LDH@PbO2 obtained in Example 1 were respectively - 1 KOH + 0.5 mol L -1 NaCl (left) and 1.0 mol L -1 Comparison of the corrosion polarization curves and the corresponding corrosion potential and corrosion current bar graphs in KOH+natural seawater (right). It can be seen from the figure that in alkaline simulated seawater and alkaline natural seawater, the corrosion potentials of the NiFe-LDH@PbO2 electrode are 1.127 and 1.1079 V, respectively, which are significantly higher than the corresponding 0.977 and 0.923 V of the NiFe-LDH electrode; the corrosion currents of the NiFe-LDH@PbO2 electrode are 1.19×10 -6 and 8.904×10 -7 Acm-2 , which is significantly lower than the 3.65×10 -6 and 2.073×10 -6 A cm -2 The corrosion data clearly show that the NiFe-LDH@PbO2 electrode has higher seawater corrosion resistance than NiFe-LDH due to the loading of PbO2 dense nanofilm.

Claims

1. A NiFe-LDH loaded PbO2 composite catalyst, characterized in that The catalyst is a composite structure formed by depositing a dense film composed of PbO2 nanoparticles on a NiFe-LDH sheet; the PbO2 nanofilm in the catalyst is prepared by constant current deposition technology under the conditions of optimal deposition time, current density and supporting electrolyte concentration; the catalyst is in-situ grown on nickel foam, and is recorded as NiFe-LDH@PbO2; The method for preparing the NiFe-LDH-loaded PbO2 composite catalyst comprises the following specific steps: (a) Preparation of NiFe-LDH The size is 2×3cm 2 The sheet-like nickel foam was placed in 3M HCl, deionized water, and anhydrous ethanol in turn, and ultrasonically treated for 15 minutes each, rinsed with deionized water for several times, and dried in an oven at 50°C; 1mmol of Ni(NO3)2·6H2O, 0.5mmol of Fe(NO3)3·9H2O, and 5mmol of urea were dissolved in 30mL of deionized water, and the mixed solution and the treated nickel foam were transferred to an 80mL polytetrafluoroethylene autoclave, reacted at 120°C for 12 hours, and the nickel foam was taken out after cooling to room temperature, and washed with ultrapure water and ethanol for several times, respectively, and dried naturally at 50°C to obtain NiFe-LDH; (b) Preparation of NiFe-LDH@PbO2 The NiFe-LDH prepared in step (a) was cut into 1×2 cm 2 specifications, using it as the working electrode, Pt wire as the counter electrode, and Ag / AgCl electrode as the reference electrode. The concentration is 100 mmol L -1 The concentration of NaNO3 is 5~200mmol L -1 The Pb(NO3)2 mixed solution is used as the electrolyte, and the current density is 5-30mA -2 , a constant current deposition is performed under the condition of a deposition time of 60 to 1800 s to grow a PbO2 film on its surface. After the deposition is completed, the working electrode is removed and rinsed with deionized water, and then dried in an oven at 50°C to obtain an electrocatalyst NiFe-LDH@PbO2; In the NiFe-LDH loaded PbO2 composite catalyst, PbO2 is covered on the surface of NiFe-LDH nanosheets in the form of a film formed by connecting nanoparticles. The particle size of the PbO2 nanoparticles is less than 5nm and the thickness is less than 3nm. The lateral size of the NiFe-LDH nanosheets is 200-350nm and the thickness is 20-30nm.

2. A NiFe-LDH loaded PbO2 composite catalyst according to claim 1, characterized in that The catalyst is used in the electrocatalytic process of alkaline seawater oxidation; specifically, the catalyst NiFe-LDH@PbO2 is used in 1 mol L -1 KOH and 2.5 mol L -1 In the aqueous solution of NaCl, the dense nanofilm formed by PbO2 nanoparticles covering the surface of NiFe-LDH nanosheets can selectively inhibit the entry of chloride ions into the surface of NiFe-LDH nanosheets. -2 After 150 hours of chronopotentiometry under a current density of , the catalytic performance showed little attenuation, and the catalyst structure and substrate framework remained basically intact. However, NiFe-LDH broke after only 2 hours of chronopotentiometry under the same conditions.

Citation Information

Cited By

  • Preparation method of gluconic acid modified oxygen evolution electrocatalyst and application of gluconic acid modified oxygen evolution electrocatalyst in catalysis of seawater oxidation

    CN121802470A