SO42-Ni3S2-NiOOH catalyst electrode, preparation method and application of SO42-Ni3S2-NiOOH catalyst electrode in catalytic oxidation of furfural

By loading SO42-Ni3S2-NiOOH on the nickel foam of the carrier, efficient matching synergy is formed, and the problem of kinetic rate mismatch of nickel-based catalysts in NOR is solved, rapid dynamic equilibrium and high-efficiency reaction are achieved, and the nickel-based catalysts are broken through. Application bottleneck.

CN118910666AActive Publication Date: 2024-11-08ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153631.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The performance improvement of nickel-based catalysts in nucleophilic oxidation reaction (NOR) is limited by competing with the anode oxygen evolution reaction (OER), resulting in a mismatch in kinetic rates and making it difficult to form an efficient dynamic equilibrium.

Method used

A SO42-Ni3S2-NiOOH catalyst electrode was designed, and SO42-Ni3S2-NiOOH with a single layer heterostructure supported on nickel foam was prepared by hydrothermal reaction and electrolytic reaction to form efficient matching and coordination and rapid dynamic equilibrium.

Benefits of technology

It achieves efficient dynamic balance in the NOR process, avoids surface competition reactions of nickel-based catalysts, improves reaction rate and selectivity, breaks through the application bottleneck of nickel-based catalysts, and has simple preparation methods, low cost and few by-products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910666A_ABST
    Figure CN118910666A_ABST
Patent Text Reader

Abstract

The invention provides a SO42-Ni3S2-NiOOH catalyst electrode, a preparation method of the SO42-Ni3S2-NiOOH catalyst electrode, and an application of the SO42-Ni3S2-NiOOH catalyst electrode in furfural oxidation. The preparation method comprises the following steps: firstly, preparing a precursor Ni3S2 by taking nickel nitrate hexahydrate, thiosemicarbazide and urea as raw materials; and then the precursor Ni3S2 is placed in a three-electrode system to be subjected to an electrolytic reaction, and the catalyst electrode SO42-Ni3S2 / NF-NiOOH is obtained. According to the catalyst, in the oxidation reaction process, # imgabs0 forms efficient matching synergy, rapid dynamic balance is formed, the situation that NOR and OER competitive reaction is formed on the surface of the nickel-based catalyst is avoided, and the application bottleneck of the nickel-based catalyst in NOR is broken through. The catalytic electrode can quickly oxidize furfural into an important organic intermediate furoic acid under the electro-catalysis effect, and is high in efficiency and good in selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of catalytic technology. Specifically, it relates to a SO4 2- -Ni3S2-NiOOH catalyst electrode, preparation method and application in catalytic oxidation of furfural. Background Art

[0002] Using renewable energy (e.g., wind, solar, and tidal energy) to drive water splitting to produce hydrogen (H2) is a promising solution to the environmental and energy challenges brought about by the continued use of fossil fuels. However, the slow four-electron transfer of the anodic oxygen evolution reaction (OER) leads to high energy consumption, consuming 95% of the total energy in the water splitting process. Replacing OER with the oxidation reaction (NOR) of nucleophiles (e.g., hydroxyls, aldehydes, amines, and alcohols) can reduce energy consumption and produce value-added chemicals. NOR is considered to be the most promising alternative to OER and has received widespread attention. The oxidation process of nucleophiles (e.g., glycerol, glucose, urea, amines, hydrazine hydrate, etc.) is a complex process involving proton-coupled electron transfer (PCET) processes, hydration processes, intramolecular rearrangements, etc., among which the PCET process is the key step. However, improving the NOR performance by regulating the dehydrogenation step in the PCET process remains a challenge.

[0003] At present, various methods (introducing elements that induce oxygen affinity, constructing heterostructures, embedding methods, doping, oxygen lattice mismatch, and constructing vacancies, etc.) have been reported to improve the performance of NOR by increasing the Fermi level and broadening the d-band width. However, since NOR and OER have similar active centers, the accumulation of active centers on the catalyst surface will improve the performance of OER, thereby forming a competitive reaction, which greatly limits the application prospects of nickel-based catalysts in NOR electrocatalysis. The bottleneck of nickel-based catalysts in improving the performance of NOR makes it impossible to effectively match the deprotonation kinetic rate of the catalyst and the dehydrogenation oxidation kinetic rate of the nucleophile. Based on the above challenges, the present invention designs a new catalyst that makes An efficient matching synergy is formed, and a rapid dynamic balance is achieved during the NOR process. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a SO4 2- -Ni3S2-NiOOH catalyst electrode, preparation method and application in furfural oxidation. The catalyst is used in the NOR process An efficient matching synergy is formed, and a rapid dynamic balance is formed. The catalytic electrode can quickly oxidize furfural into an important organic intermediate furoic acid under the action of electrocatalysis, with high efficiency and good selectivity.

[0005] The present invention is achieved through the following technical solutions

[0006] First, the present invention provides a SO4 2- -Ni3S2-NiOOH catalyst electrode, the electrode comprising:

[0007] Carrier nickel foam;

[0008] Single-layer heterostructure SO4 loaded on a carrier 2- -Ni3S2-NiOOH.

[0009] The present invention also provides the above-mentioned SO4 2- - A method for preparing a Ni3S2-NiOOH catalyst electrode, the method comprising the following steps:

[0010] (1) nickel nitrate hexahydrate, thiosemicarbazide and urea are prepared into a solution, mixed evenly and placed in a high-pressure reactor; nickel foam is leached into the high-pressure reactor to perform a hydrothermal reaction, and after the reaction is completed, cooled, washed and dried to obtain a precursor Ni3S2;

[0011] (2) The precursor Ni3S2 obtained in step (1) is placed in a three-electrode system for electrolysis reaction, and the catalyst electrode SO4 is obtained after the reaction is completed. 2- -Ni3S2-NiOOH.

[0012] Furthermore, in step (1), the molar ratio of nickel nitrate hexahydrate, thiosemicarbazide and urea is 1-3:1-3:1-3;

[0013] And / or the solvent for preparing the solution is preferably deionized water.

[0014] Furthermore, the temperature of the hydrothermal reaction in step (1) is 120-200° C. and the reaction time is 9-14 h.

[0015] Furthermore, in the electrolysis reaction described in step (2), the voltage is 1.4 to 1.8 V, and the electrolysis time is 5 to 60 min.

[0016] Furthermore, the drying temperature in step (1) is 50-70° C. and the drying time is 4-8 hours.

[0017] Furthermore, the three electrodes described in step (2) are specifically: working electrode: Ni3S2 catalytic electrode; counter electrode: graphite rod; reference electrode: Ag / AgCl electrode.

[0018] Furthermore, the nickel foam in step (1) is ultrasonically treated with acetone, hydrochloric acid and deionized water before leaching; and / or the concentration of the hydrochloric acid is 3M;

[0019] And / or the ultrasonic treatment time is 10 minutes.

[0020] The present invention also provides the use of the above-mentioned catalyst electrode in the electro-oxidation of furfural to produce furanic acid. The catalyst electrode has good selectivity in the electro-catalytic oxidation of furfural, the yield of furfural obtained by oxidation of furfural is high, and the cyclic stability of the reaction is good. Thus, the problems existing in the prior art are solved, and a catalyst construction strategy is provided for effectively improving the performance of nucleophilic reagents in electro-catalytic oxidation, which has good application prospects. The obtained furanic acid is an important intermediate in organic synthesis and has good economic benefits.

[0021] The present invention has the following positive beneficial effects

[0022] The catalyst electrode prepared by the present invention has good reaction rate and selectivity in the oxidation reaction (NOR) of nucleophilic reagents, and can quickly reach equilibrium during the process, that is, form a rapid dynamic equilibrium, thereby avoiding the competitive reaction between NOR and OER formed on the surface of the nickel-based catalyst, and breaking through the application bottleneck of the nickel-based catalyst in NOR.

[0023] The catalyst preparation method is simple and easy, does not use or produce toxic substances, has low cost, high yield, and few by-products, and the obtained catalyst electrode has good application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of the catalyst electrode prepared in Example 1;

[0025] Figure 2 Elemental mapping of the catalyst electrode prepared in Example 1;

[0026] Figure 3 Preparation of catalyst electrode SO4 for Example 1 2- -Ni 2p XPS spectrum of Ni3S2-NiOOH;

[0027] Figure 4 Preparation of catalyst electrode SO4 for Example 1 2- -S2p XPS spectrum of Ni3S2-NiOOH;

[0028] Figure 5 This is a Raman spectrum of the catalyst electrode prepared in Example 1;

[0029] Figure 6 NiO / NF, Ni(OH)2 / NF and SO4 prepared in Example 1 2- -Ni3S2-NiOOH at a rate of 5 mV s in 1.0 M KOH, 1.0 M KOH, and 50 mM furfural (FF) -1 Linear sweep saturation (LSV) curve when ;

[0030] Figure 7 NiO / NF, Ni(OH)2 / NF and SO4 prepared in Example 1 2- -Ni3S2-NiOOH three catalyst electrodes under 1.0M KOH condition, with or without 50mM furfural (FF), 5mV s -1 Tafel slope plot (Tafel);

[0031] Figure 8 NiO / NF, Ni(OH)2 / NF and prepared SO4 2- - Yield diagram of the electrolytic oxidation of furfural to furanoic acid using three catalyst electrodes, Ni3S2-NiOOH, under 1.0M KOH conditions;

[0032] Fig. 9 NiO / NF, Ni(OH)2 / NF and prepared SO4 2- -Production rate diagram of furfural electrolysis oxidation on three catalyst electrodes: Ni3S2-NiOOH;

[0033] Fig.10 SO4 2- -FE and yield results of furfural (FF) electrooxidation over Ni3S2-NiOOH catalyst;

[0034] Fig.11 SO4 2- -Ni3S2-NiOOH catalyst at 1.60V RHE Graph showing the cyclic stability experimental results of FE and yield of electro-oxidation furfural (FF);

[0035] Fig.12 For the two-electrode flow electrochemical cell SO4 2- - Yield and Faraday efficiency of furfural (FF) electrooxidation over Ni3S2-NiOOH catalyst;

[0036] Fig.13 For the two-electrode flow electrochemical cell SO4 2- -Stability test diagram of Ni3S2-NiOOH catalyst electro-oxidation of furfural (FF). DETAILED DESCRIPTION

[0037] The present invention is described in more detail below through specific implementation methods to facilitate understanding of the technical solution of the present invention, but is not intended to limit the protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0038] It should be noted that hydrochloric acid (HCl, ≥37%), ethanol (≥99.7%), nickel nitrate hexahydrate (Ni(NO3)26H2O), urea, thiosemicarbazide (CH4N2S), potassium hydroxide (KOH), and furfural (FF) were purchased from Aldrich (China). All reagents were used without purification. Nickel foam (NF) was provided by HGP.

[0039] Example 1

[0040] SO4 2- - A method for preparing a Ni3S2-NiOOH catalyst electrode, the method comprising the following steps:

[0041] (1) ultrasonically cleaning the nickel foam with acetone, 3 mol / L hydrochloric acid, and deionized water in sequence to obtain a pretreated nickel foam;

[0042] (2) 3 mmol of nickel nitrate hexahydrate, 3 mmol of thiosemicarbazide and 9 mmol of urea were dissolved in 30 ml of deionized water and stirred for 30 min. After mixing evenly, the mixture was placed in a 50 ml high pressure reactor;

[0043] Then, the nickel foam treated in step (1) is leached into a high-pressure reactor, subjected to a hydrothermal reaction at 180° C. for 12 h, and after the reaction is completed, cooled, washed, and vacuum dried at 60° C. for 6 h to obtain a precursor;

[0044] (3) The precursor obtained in step (2) was placed in a three-electrode system for electrolysis reaction (the three electrodes are: working electrode: Ni3S2 catalytic electrode; counter electrode: graphite rod; reference electrode: Ag / AgCl electrode), and electrolysis was performed at a voltage of 1.6 V for 30 min to obtain the catalyst electrode SO4 2- -Ni3S2-NiOOH.

[0045] Example 2

[0046] SO4 2- - A method for preparing a Ni3S2-NiOOH catalyst electrode, the method comprising the following steps:

[0047] (1) ultrasonically cleaning the nickel foam with 3 mol / L hydrochloric acid, anhydrous ethanol, and deionized water in sequence to obtain a pretreated nickel foam;

[0048] (2) 9 mmol of nickel nitrate hexahydrate, 3 mmol of thiosemicarbazide and 3 mmol of urea were dissolved in 30 ml of deionized water and stirred for 30 min. After mixing evenly, the mixture was placed in a 50 ml high pressure reactor;

[0049] Then, the nickel foam treated in step (1) is leached into a high-pressure reactor, subjected to a hydrothermal reaction at 180° C. for 12 h, and after the reaction is completed, cooled, washed, and vacuum dried at 60° C. for 6 h to obtain a precursor;

[0050] (3) The precursor obtained in step (2) is placed in a three-electrode system for electrolysis reaction, wherein the three electrodes are specifically a working electrode: a Ni3S2 catalytic electrode; a counter electrode: a graphite rod; and a reference electrode: an Ag / AgCl electrode. The electrolysis is performed at a voltage of 1.6 V for 30 min to obtain a catalyst electrode SO4 2- -Ni3S2-NiOOH.

[0051] Example 3

[0052] SO4 2- - A method for preparing a Ni3S2-NiOOH catalyst electrode, the method comprising the following steps:

[0053] (1) ultrasonically cleaning the nickel foam with acetone, 3 mol / L hydrochloric acid, and deionized water in sequence to obtain a pretreated nickel foam;

[0054] (2) 3 mmol of nickel nitrate hexahydrate, 9 mmol of thiosemicarbazide and 3 mmol of urea were dissolved in 30 ml of deionized water and stirred for 30 min. After mixing evenly, the mixture was placed in a 50 ml high pressure reactor;

[0055] Then, the nickel foam treated in step (1) is leached into a high-pressure reactor, subjected to a hydrothermal reaction at 180° C. for 12 h, and after the reaction is completed, cooled, washed, and vacuum dried at 60° C. for 6 h to obtain a precursor;

[0056] (3) The precursor obtained in step (2) is placed in a three-electrode system for electrolysis reaction, wherein the three electrodes are specifically a working electrode: a Ni3S2 catalytic electrode; a counter electrode: a graphite rod; and a reference electrode: an Ag / AgCl electrode. The electrolysis is performed at a voltage of 1.6 V for 30 min to obtain a catalyst electrode SO4 2- -Ni3S2-NiOOH.

[0057] Example 4

[0058] SO4 2- - A method for preparing a Ni3S2-NiOOH catalyst electrode, the method comprising the following steps:

[0059] (1) ultrasonically cleaning the nickel foam with acetone, 3 mol / L hydrochloric acid, and deionized water in sequence to obtain a pretreated nickel foam;

[0060] (2) 3 mmol of nickel nitrate hexahydrate, 3 mmol of thiosemicarbazide and 9 mmol of urea were dissolved in 30 ml of deionized water and stirred for 30 min. After mixing evenly, the mixture was placed in a 50 ml high pressure reactor;

[0061] Then, the nickel foam treated in step (1) is leached into a high-pressure reactor, subjected to a hydrothermal reaction at 180° C. for 12 h, and after the reaction is completed, cooled, washed, and vacuum dried at 60° C. for 6 h to obtain a precursor;

[0062] (3) The precursor obtained in step (2) was placed in a three-electrode system for electrolysis reaction (the three electrodes are: working electrode: Ni3S2 catalytic electrode; counter electrode: graphite rod; reference electrode: Ag / AgCl electrode), and electrolysis was performed at a voltage of 1.4 V for 30 min to obtain the catalyst electrode SO4 2- -Ni3S2-NiOOH.

[0063] Example 5

[0064] SO4 2- - A method for preparing a Ni3S2-NiOOH catalyst electrode, the method comprising the following steps:

[0065] (1) ultrasonically cleaning the nickel foam with acetone, 3 mol / L hydrochloric acid, and deionized water in sequence to obtain a pretreated nickel foam;

[0066] (2) 3 mmol of nickel nitrate hexahydrate, 3 mmol of thiosemicarbazide and 9 mmol of urea were dissolved in 30 ml of deionized water and stirred for 30 min. After mixing evenly, the mixture was placed in a 50 ml high pressure reactor;

[0067] Then, the nickel foam treated in step (1) is leached into a high-pressure reactor, subjected to a hydrothermal reaction at 180° C. for 12 h, and after the reaction is completed, cooled, washed, and vacuum dried at 60° C. for 6 h to obtain a precursor;

[0068] (3) The precursor obtained in step (2) was placed in a three-electrode system for electrolysis reaction (the three electrodes are: working electrode: Ni3S2 catalytic electrode; counter electrode: graphite rod; reference electrode: Ag / AgCl electrode), and electrolysis was performed at a voltage of 1.5 V for 30 min to obtain the catalyst electrode SO4 2- -Ni3S2-NiOOH.

[0069] The catalyst prepared in the above example was tested for performance:

[0070] (1) First, the structure and composition of the catalyst are tested, as follows:

[0071] The morphology and structure of the samples were determined by scanning electron microscopy (SEM). Figure 1 As shown, the NF surface is vertically grown SO4 2- -Ni3S2-NiOOH nanosheets coverage.

[0072] SO4 2- -Elemental mapping of Ni3S2-NiOOH catalyst electrode Figure 2 As shown, Ni, S, and O elements are evenly distributed throughout the nanosheets.

[0073] XPS spectrum was used to analyze the changes in the valence states of Ni 2p, O 2p and S2p during the process. Figure 3 As shown, the peaks at 854.92 eV and 872.72 eV are attributed to Ni 2+ / Ni 3+ 2p 3 / 2 and 2p 1 / 2 , while the peaks at 862.33eV and 879.86eV are attributed to satellite peaks. This shows that SO4 2- -Ni3S2-NiOOH contains Ni 3+ .

[0074] The XPS spectrum of S shows Figure 4 As shown, SO4 2- -There is obvious SO4 in the S2p XPS spectrum of Ni3S2-NiOOH 2- (~169.7eV).

[0075] Figure 5 This is the Raman spectrum of the catalyst electrode of Example 1. From the Raman spectrum, it can be seen that Ni3S2 / NF does not contain NiOOH and SO4 2- The Raman signal of the prepared product is 480cm -1 and 550cm -1 The Raman peak at 980 cm-1 indicates the formation of NiOOH. -1 The Raman peak at 2- This is consistent with the XPS results. Based on the above characterization, it can be seen that the final catalyst structure is SO4 2- -Ni3S2-NiOOH.

[0076] (2) Then the application performance of the catalyst electrode (furfural oxidation reaction (FOR)) was tested as follows: The catalyst electrode SO4 prepared in the above embodiment was taken 2- -Ni3S2-NiOOH, NiO / NF, Ni(OH)2 / NF, 1X1cm 2The working electrode was placed in a three-electrode system (counter electrode: graphite rod; reference electrode: Ag / AgCl electrode) and the rate was 5 mV s at 1.0 M KOH, 1.0 M KOH, and 50 mM furfural (FF), respectively. -1 The linear sweep (LSV) curve is as follows Figure 6 As shown. SO4 2- -Ni3S2-NiOOH has better catalytic activity for FOR than Ni(OH)2 / NF and NiO / NF.

[0077] NiO / NF, Ni(OH)2 / NF and SO4 2- -Ni3S2-NiOOH three catalyst electrodes under 1.0M KOH condition, with or without 50mM furfural (FF), 5mV s -1 The Tafel slope diagram (Tafel) is as follows Figure 7 As shown; SO4 2- -The Tafel slope value of Ni3S2-NiOOH is 34mV dec -1 , much lower than Ni(OH)2 / NF(78mV dec -1 ) and NiO / NF (126mV dec -1 ), indicating SO4 2- -Ni3S2-NiOOH has a faster reaction rate.

[0078] NiO / NF, Ni(OH)2 / NF and SO4 2- The yield of furanic acid (FA) from the electrolytic oxidation of 50 mM furfural (FF) (electrolysis for 30 min) using three catalyst electrodes -Ni3S2-NiOOH under 1.0 M KOH is shown in the figure. Figure 8 As shown, SO4 2- -The FA yield of Ni3S2-NiOOH is significantly higher than that of Ni(OH)2 / NF and NiO / NF. RHE to 1.60V RHE FA production increases with the increase of applied potential. RHE The highest output.

[0079] NiO / NF, Ni(OH)2 / NF and SO4 2- -Ni3S2-NiOOH three catalyst electrodes under 1.0M KOH conditions, furfural oxidation reaction (FOR) 30min production rate diagram as shown Fig. 9 As shown in the figure, SO4 2- The rate of furoic acid (FA) production after the electrocatalytic furfural oxidation reaction (FOR) of -Ni3S2-NiOOH was significantly higher than that of Ni(OH)2 / NF and NiO / NF.

[0080] SO4 2- -The Faraday efficiency (FE) and yield (Yield) of furfural (FF) after 30 min of electrooxidation over Ni3S2-NiOOH catalyst are shown in Fig.10 As shown in the figure, SO4 2- -Ni3S2-NiOOH FA yield is significantly higher than that of Ni(OH)2 / NF and NiO / NF. When the applied voltage is 1.6V RHE When , the FE and yield of FOR reached 90% and 70%, respectively.

[0081] SO4 2- -Ni3S2-NiOOH catalyst at 1.60V RHE The cyclic stability test results of FE and yield of furfural (FF) after 30 min of electrooxidation are shown in Figure 2. Fig.11 As shown in the figure, it can be seen that SO4 2- -Ni3S2-NiOOH maintained good yield and Faraday efficiency after 6 cycles in the FOR process, indicating that SO4 2- -Ni3S2-NiOOH has high stability.

[0082] (3) The present invention further studies SO4 using a double-electrode electrochemical flow cell 2- -FOR||HER performance of Ni3S2-NiOOH. Among them, SO4 2- -Ni3S2-NiOOH serves as both anode and cathode catalyst.

[0083] The yield and Faraday efficiency of furfural (FF) oxidation in a two-electrode flow electrochemical cell are shown in the figure. Fig.12 As shown, the conversion rate of FA is 44% to 70%, and the conversion rate of FE is 70%. In the range of 1.40V to 1.60V, the FE value of the electrochemical flow cell is between 95% and 98%.

[0084] Fig.13 The stability test of the two-electrode flow electrochemical cell at 1.60V for 30h showed that the voltage change was not obvious, indicating that SO4 2- -Ni3S2-NiOOH has good stability in flow batteries.

Claims

1. A A method for preparing a catalyst electrode, characterized in that: The method comprises the following steps: (1) nickel nitrate hexahydrate, thiosemicarbazide and urea are prepared into a solution, mixed evenly and placed in a high-pressure reactor, nickel foam is leached into the high-pressure reactor, a hydrothermal reaction is carried out, and after the reaction is completed, the precursor is cooled, washed and dried; (2) placing the precursor obtained in step (1) in a three-electrode system for electrolysis reaction, and obtaining a catalyst electrode after the reaction is completed 2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of nickel nitrate hexahydrate, thiosemicarbazide and urea is 1-3:1-3:1-3; And / or the solvent used to prepare the solution is preferably deionized water.

3. The preparation method according to claim 1 or 2, characterized in that: The temperature of the hydrothermal reaction in step (1) is 120-200° C. and the reaction time is 9-14 hours.

4. The preparation method according to claim 1 or 2, characterized in that: In the electrolysis reaction of step (2), the voltage is 1.4 to 1.8 V and the electrolysis time is 5 to 60 min.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The drying temperature in step (1) is 50-70° C. and the drying time is 4-8 hours.

6. The preparation method according to any one of claims 1 to 4, characterized in that: The three electrodes described in step (2) are: working electrode: Ni3S2 catalytic electrode; counter electrode: graphite rod; reference electrode: Ag / AgCl electrode.

7. The preparation method according to any one of claims 1 to 4, characterized in that: The nickel foam in step (1) is subjected to ultrasonic treatment using acetone, hydrochloric acid and deionized water in sequence before leaching; And / or the concentration of the hydrochloric acid is 3M.

8. A catalyst electrode prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The electrode includes a carrier nickel foam; Single-layer heterostructure loaded on a carrier 9. Use of the catalyst electrode according to any one of claims 1 to 8 in the electro-oxidation of furfural.