Rapid growth method of high-quality and high-purity piezoelectric crystal
By using ultrasonic cleaning technology combined with silicon-containing Gemini surfactant and hydrochloric acid solution, the problem of impurity removal in natural quartz stone is solved, the growth rate and quality of piezoelectric crystal is improved, and high-quality and high-purity piezoelectric crystal is achieved. Production.
Patent Information
- Application Number
- CN202410956744.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when manufacturing high-quality and high-purity piezoelectric crystals, it is difficult to effectively remove impurities in natural quartz stone, which affects the growth rate and quality of crystals. In addition, traditional washing powder surfactants have adsorption film residues and ion binding during the cleaning process. Problem affecting the cleaning effect.
Silicon-containing Gemini surfactant is used to combine with hydrochloric acid solution to remove impurities in natural quartz stone through ultrasonic treatment, and the impurities are exposed and broken through heating and quenching treatment. Combined with ultrasonic and quenching cycle cleaning, the cleaning effect is further improved.
Effectively remove impurities in natural quartz stone, improve the growth rate and quality of piezoelectric crystals, reduce internal defects, and obtain high frequency stability and low defects piezoelectric crystals, meeting the requirements of high-precision electronic component manufacturing.
Smart Images

Figure CN118910734A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of piezoelectric crystal manufacturing, and in particular relates to a method for rapidly growing high-quality and high-purity piezoelectric crystal. Background Art
[0002] Piezoelectric crystal (piezoquartz), also known as piezoelectric quartz, refers to a crystal single crystal with piezoelectric effect. In the crystal used as the raw material of the piezoelectric crystal industry, defects that affect the piezoelectric effect, such as Dauphin twins, Brazilian twins, nodules, cracks, cotton, inclusions (solid, gas, liquid), etc., are not allowed to exist. High-precision, high-ratio piezoelectric crystal components (such as resonators, filters, etc.) made of this single crystal have the highest frequency stability. The piezoelectric crystals currently used are divided into natural crystals and artificial crystals, but impurities are inevitably present in natural crystals, which affect the performance of piezoelectric crystals. At present, artificial crystal growth generally adopts the hydrothermal temperature difference method in a sealed autoclave. In order to produce artificial crystal single crystals that are colorless, transparent, free of impurities, cracks and other defects, and meet certain geometric size requirements, the requirements for the crystal growth method are relatively high. The current process uses natural quartz stone as a culture medium. If the quartz stone contains impurities, these impurities will spread during the crystal growth process, causing the quality of the entire crystal to decline and affecting the growth rate of the crystal. The purity of the quartz stone will affect the crystal growth rate. High-purity quartz stone can promote a more uniform growth rate, and high-purity quartz stone helps to grow larger crystals because the reduction in impurities also reduces problems that may occur during the crystal growth process, such as crystal breakage or growth interruption.
[0003] The Chinese invention patent with the authorization announcement number CN101275273B discloses a method for manufacturing piezoelectric crystals, using granular natural quartz as a culture medium, but the invention only simply cleans the natural quartz and does not mention the specific cleaning process of the natural quartz. The Chinese invention patent with the publication number CN103938271A discloses a method for growing piezoelectric crystals, which uses washing powder to remove impurities on the surface of natural quartz, and then puts the cleaned quartz into an autoclave to grow piezoelectric crystals. The main component of washing powder is anionic surfactants, which are easy to form adsorption films on the surface of the washed object and remain on the object, affecting the removal of impurities, and anionic surfactants are also easy to combine with calcium, magnesium and other ions, thereby affecting the cleaning effect. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a method for rapid growth of high-quality and high-purity piezoelectric crystal. This method effectively removes impurities in natural quartz stone through special cleaning and growth steps, improves the rate and quality of crystal growth, and thus obtains piezoelectric crystal single crystals with high frequency stability and low internal defects.
[0005] In order to achieve the above object, the following technical scheme is adopted: The present invention provides a method for rapidly growing high-quality and high-purity piezoelectric crystal, comprising the following steps:
[0006] S1. Mix terminal allyl polyether and diglycolic anhydride, introduce nitrogen, heat to 50-60° C., add hydroxypropyl-terminated polydimethylsiloxane and tricyclohexylphosphine, stir evenly, and finally add diallyl isocyanurate and palladium acetate to obtain a silicon-containing Gemini surfactant;
[0007] S2, after natural quartz stone is sorted, it is washed with deionized water to remove surface impurities, and then the sorted natural quartz stone is placed in a trough, the trough is immersed in a hydrochloric acid solution, and then the silicon-containing Gemini surfactant is added, and the hydrochloric acid solution is ultrasonically treated by an ultrasonic device. After 10-20 minutes, the trough is taken out, and the trough is quickly immersed in deionized water at room temperature for rapid cooling, and the ultrasonic and rapid cooling process is repeated again. The obtained quartz material is crushed and sieved, and the quartz crushed material with a diameter of 1.5-3cm is selected as the culture body, and is placed in the lower part of the autoclave;
[0008] S3, high-purity water is loaded into the autoclave, the piezoelectric crystal is cut along the c direction to obtain the Z-axis seed crystal, the Z-axis seed crystal is placed in a hydrofluoric acid solution and soaked for 4-5 hours, then washed with deionized water, and then cut and punched, the seed crystal is hung on a seed crystal rack, and then the seed crystal rack is loaded into the autoclave, an isolation plate is set on the seed crystal rack, and convection holes are set on the isolation plate, and then the autoclave is sealed;
[0009] S4, start the autoclave, perform programmed temperature control on the upper and lower parts of the autoclave respectively, and obtain the piezoelectric crystal after maintaining the temperature and pressure for 50-55 days.
[0010] Furthermore, the feeding mass ratio of the terminal allyl polyether, diglycolic anhydride, hydroxypropyl-terminated polydimethylsiloxane, tricyclohexylphosphine, diallyl isocyanurate and palladium acetate is 80-120:10-15:120-150:1-5:20-30:1-5.
[0011] Furthermore, the mass fraction of the hydrochloric acid solution is 10%-20%.
[0012] Furthermore, the amount of the silicon-containing Gemini surfactant is 1%-5% of the mass of the hydrochloric acid solution.
[0013] Furthermore, the ultrasonic treatment has a power of 20-35 W / L and a temperature of 60-80°C.
[0014] Furthermore, the mass fraction of the hydrofluoric acid solution is 20%-30%.
[0015] Furthermore, the filling degree of the high-purity water is 75%-85%.
[0016] Furthermore, the diameter of the convection holes on the isolation plate is 15-30 mm, and the opening rate of the isolation plate is 4%-8%.
[0017] Furthermore, the pressure of the autoclave is 140-160 MPa.
[0018] Further, the upper part of the autoclave is heated to 100-110°C at 4°C / min, kept at this temperature for 4 hours, then heated to 230-250°C at 4°C / min, kept at this temperature for 20 hours, and then heated to 320-340°C at 4°C / min, and kept at this temperature until the growth is completed;
[0019] Furthermore, the upper part of the autoclave is heated to 120-130°C at 4°C / min, kept warm for 4 hours, then heated to 260-270°C at 4°C / min, kept warm for 20 hours, and then heated to 340-360°C at 4°C / min, and kept warm until the growth is completed.
[0020] The beneficial effects of the present invention are:
[0021] (1) The present invention prepares a silicon-containing Gemini surfactant. Compared with traditional detergent surfactants, the Gemini surfactant has a lower critical micelle concentration, can more effectively reduce surface tension, and has a better cleaning effect. The present invention uses the Gemini surfactant together with a hydrochloric acid solution and cleans natural quartz stone by ultrasonic treatment. The ultrasonic treatment causes agitation between the quartz stone and the hydrochloric acid solution, which accelerates the chemical reaction rate between the quartz stone and the acid, thereby quickly removing impurities in the natural quartz stone;
[0022] (2) The silicon-containing Gemini surfactant prepared by the present invention has good water solubility and salt resistance, and the organic silicon and isocyanurate contained therein are acid-resistant and temperature-resistant, and will not be affected by the cleaning environment and temperature changes to reduce the cleaning effect;
[0023] (3) The present invention heats the quartz stone first and then quenches it with deionized water, so that cracks are generated when the temperature changes suddenly, thereby fully exposing the impurities contained therein, providing more contact area for the subsequent cleaning steps, and combining Gemini surfactant, hydrochloric acid solution and ultrasonic treatment to achieve deeper impurity removal, and also promote the subsequent crushing and screening of natural quartz stone;
[0024] (4) The method of the present invention not only improves the growth rate of piezoelectric crystal and shortens the production cycle, but also optimizes the quality of piezoelectric crystal by precisely controlling the growth conditions. The obtained piezoelectric crystal has a higher Q value, lower internal defects and corrosion tunnel density. The obtained piezoelectric crystal has the advantages of high quality and high purity, meeting the strict requirements of high-precision electronic component manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 XRD images of Examples 1-3 of a method for rapid growth of high-quality and high-purity piezoelectric crystals according to the present invention;
[0026] Figure 2 The Q values of various embodiments and comparative examples of a method for rapidly growing high-quality and high-purity piezoelectric crystals of the present invention are shown in FIG.
[0027] Figure 3 The density of the corrosion tunnels in various embodiments and comparative examples of a method for rapid growth of high-quality and high-purity piezoelectric crystals of the present invention;
[0028] Figure 4 The total impurity content of each embodiment and comparative example of a method for rapid growth of high-quality and high-purity piezoelectric crystal of the present invention.
[0029] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0032] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0033] Example 1
[0034] A rapid growth method for high-quality and high-purity piezoelectric crystal
[0035] The growth method comprises the following steps:
[0036] S1. Mix terminal allyl polyether and diglycolic anhydride, introduce nitrogen, heat to 50° C., add hydroxypropyl-terminated polydimethylsiloxane and tricyclohexylphosphine, stir evenly, and finally add diallyl isocyanurate and palladium acetate to obtain a silicon-containing Gemini surfactant;
[0037] S2, after natural quartz stone is sorted, it is washed with deionized water to remove surface impurities, and then the sorted natural quartz stone is placed in a trough, and the trough is immersed in a hydrochloric acid solution with a mass fraction of 10%, and then the silicon-containing Gemini surfactant is added, and the hydrochloric acid solution is ultrasonically treated by an ultrasonic device. After 10 minutes, the trough is taken out, and the trough is quickly immersed in deionized water at room temperature for rapid cooling, and the ultrasonic and rapid cooling process is repeated again. The obtained quartz material is crushed and sieved, and the quartz crushed material with a diameter of 1.5-3cm is selected as the culture body, and is placed in the lower part of the autoclave;
[0038] S3, high-purity water is filled into the autoclave with a filling degree of 75%, the piezoelectric crystal is cut along the c direction to obtain the Z-axis seed crystal, the Z-axis seed crystal is placed in a hydrofluoric acid solution with a mass fraction of 20% and soaked for 4 hours, then washed with deionized water, and then cut and punched, the seed crystal is hung on the seed crystal rack, and then the seed crystal rack is placed in the autoclave, an isolation plate is set on the seed crystal rack, and convection holes are set on the isolation plate, and then the autoclave is sealed;
[0039] S4, start the autoclave, perform programmed temperature control on the upper and lower parts of the autoclave respectively, and obtain the piezoelectric crystal after maintaining the temperature and pressure for 55 days.
[0040] The feeding mass ratio of the terminal allyl polyether, diglycolic anhydride, hydroxypropyl-terminated polydimethylsiloxane, tricyclohexylphosphine, diallyl isocyanurate and palladium acetate is 80:10:120:1:20:1.
[0041] The amount of the silicon-containing Gemini surfactant used is 1% of the mass of the hydrochloric acid solution.
[0042] The power of the ultrasonic treatment is 20 W / L and the temperature is 60°C.
[0043] The diameter of the convection holes on the isolation plate is 15 mm, and the opening rate of the isolation plate is 4%.
[0044] The pressure of the autoclave is 140 MPa.
[0045] The upper part of the autoclave was heated to 100°C at 4°C / min, kept at that temperature for 4 hours, then heated to 230°C at 4°C / min, kept at that temperature for 20 hours, and then heated to 320°C at 4°C / min, and kept at that temperature until the growth was completed;
[0046] The upper part of the autoclave was heated to 120°C at 4°C / min, kept at that temperature for 4 hours, then heated to 260°C at 4°C / min, kept at that temperature for 20 hours, and then heated to 340°C at 4°C / min, kept at that temperature until the growth was completed.
[0047] Example 2
[0048] A rapid growth method for high-quality and high-purity piezoelectric crystal
[0049] The growth method comprises the following steps:
[0050] S1. Mix terminal allyl polyether and diglycolic anhydride, introduce nitrogen, heat to 60°C, add hydroxypropyl-terminated polydimethylsiloxane and tricyclohexylphosphine, stir evenly, and finally add diallyl isocyanurate and palladium acetate to obtain a silicon-containing Gemini surfactant;
[0051] S2, after natural quartz stone is sorted, it is washed with deionized water to remove surface impurities, and then the sorted natural quartz stone is placed in a trough, and the trough is immersed in a hydrochloric acid solution with a mass fraction of 20%, and then the silicon-containing Gemini surfactant is added, and the hydrochloric acid solution is ultrasonically treated by an ultrasonic device. After 20 minutes, the trough is taken out, and the trough is quickly immersed in deionized water at room temperature for rapid cooling, and the ultrasonic and rapid cooling process is repeated again. The obtained quartz material is crushed and sieved, and the quartz crushed material with a diameter of 1.5-3cm is selected as the culture body, and is placed in the lower part of the autoclave;
[0052] S3, high-purity water is filled into the autoclave with a filling degree of 85%, the piezoelectric crystal is cut along the c direction to obtain the Z-axis seed crystal, the Z-axis seed crystal is placed in a hydrofluoric acid solution with a mass fraction of 30% and soaked for 5 hours, then washed with deionized water, and then cut and punched, the seed crystal is hung on the seed crystal rack, and then the seed crystal rack is placed in the autoclave, an isolation plate is set on the seed crystal rack, and convection holes are set on the isolation plate, and then the autoclave is sealed;
[0053] S4, start the autoclave, perform programmed temperature control on the upper and lower parts of the autoclave respectively, and obtain the piezoelectric crystal after maintaining the temperature and pressure for 53 days.
[0054] The feeding mass ratio of the terminal allyl polyether, diglycolic anhydride, hydroxypropyl-terminated polydimethylsiloxane, tricyclohexylphosphine, diallyl isocyanurate and palladium acetate is 120:15:150:5:30:5.
[0055] The amount of the silicon-containing Gemini surfactant used is 5% of the mass of the hydrochloric acid solution.
[0056] The power of the ultrasonic treatment is 35 W / L and the temperature is 80°C.
[0057] The diameter of the convection holes on the isolation plate is 30 mm, and the opening rate of the isolation plate is 8%.
[0058] The pressure of the autoclave is 160 MPa.
[0059] The upper part of the autoclave was heated to 110°C at 4°C / min, kept at this temperature for 4 hours, then heated to 250°C at 4°C / min, kept at this temperature for 20 hours, and then heated to 340°C at 4°C / min, kept at this temperature until the growth was completed;
[0060] The upper part of the autoclave was heated to 130°C at 4°C / min, kept at that temperature for 4 hours, then heated to 270°C at 4°C / min, kept at that temperature for 20 hours, and then heated to 360°C at 4°C / min, kept at that temperature until the growth was completed.
[0061] Example 3
[0062] A rapid growth method for high-quality and high-purity piezoelectric crystal
[0063] The growth method comprises the following steps:
[0064] S1, mixing terminal allyl polyether and diglycolic anhydride, introducing nitrogen, heating to 55°C, adding hydroxypropyl-terminated polydimethylsiloxane and tricyclohexylphosphine, stirring evenly, and finally adding diallyl isocyanurate and palladium acetate to obtain a silicon-containing Gemini surfactant;
[0065] S2, after natural quartz stone is sorted, it is washed with deionized water to remove surface impurities, and then the sorted natural quartz stone is placed in a trough, and the trough is immersed in a hydrochloric acid solution with a mass fraction of 15%, and then the silicon-containing Gemini surfactant is added, and the hydrochloric acid solution is ultrasonically treated by an ultrasonic device. After 15 minutes, the trough is taken out, and the trough is quickly immersed in deionized water at room temperature for rapid cooling, and the ultrasonic and rapid cooling process is repeated again. The obtained quartz material is crushed and sieved, and the quartz crushed material with a diameter of 1.5-3cm is selected as the culture body, and is placed in the lower part of the autoclave;
[0066] S3, high-purity water is filled into the autoclave with a filling degree of 80%, the piezoelectric crystal is cut along the c direction to obtain the Z-axis seed crystal, the Z-axis seed crystal is placed in a hydrofluoric acid solution with a mass fraction of 25% and soaked for 4.5 hours, then washed with deionized water, and then cut and punched, the seed crystal is hung on the seed crystal rack, and then the seed crystal rack is placed in the autoclave, an isolation plate is set on the seed crystal rack, and convection holes are set on the isolation plate, and then the autoclave is sealed;
[0067] S4, start the autoclave, perform programmed temperature control on the upper and lower parts of the autoclave respectively, and obtain the piezoelectric crystal after maintaining the temperature and pressure for 50 days.
[0068] The feeding mass ratio of the terminal allyl polyether, diglycolic anhydride, hydroxypropyl-terminated polydimethylsiloxane, tricyclohexylphosphine, diallyl isocyanurate and palladium acetate is 100:12:140:2.5:25:3.
[0069] The amount of the silicon-containing Gemini surfactant used is 3% of the mass of the hydrochloric acid solution.
[0070] The power of the ultrasonic treatment is 30 W / L and the temperature is 70°C.
[0071] The diameter of the convection holes on the isolation plate is 20 mm, and the opening rate of the isolation plate is 6%.
[0072] The pressure of the autoclave is 150 MPa.
[0073] The upper part of the autoclave was heated to 105°C at 4°C / min, kept at that temperature for 4 hours, then heated to 240°C at 4°C / min, kept at that temperature for 20 hours, and then heated to 330°C at 4°C / min, kept at that temperature until the growth was completed;
[0074] The upper part of the autoclave was heated to 125°C at 4°C / min, kept at that temperature for 4 hours, then heated to 265°C at 4°C / min, kept at that temperature for 20 hours, and then heated to 350°C at 4°C / min, kept at that temperature until the growth was completed.
[0075] Comparative Example 1
[0076] The difference between this comparative example and the embodiment is that no silicon-containing Gemini surfactant is added when cleaning the natural quartz stone, and only dilute hydrochloric acid is used. The remaining components, component contents, and steps included in the preparation process are the same as those in Example 3. The piezoelectric crystal is obtained after heat preservation and pressure maintenance for 58 days.
[0077] Comparative Example 2
[0078] The difference between this comparative example and the embodiment is that an equal amount of deionized water is used instead of the hydrochloric acid solution, and an equal amount of washing powder is used instead of the silicon-containing Gemini surfactant. The remaining components, component contents, and steps included in the preparation process are the same as those in Example 3. The piezoelectric crystal is obtained after heat preservation and pressure maintenance for 65 days.
[0079] Results Analysis
[0080] The piezoelectric crystal prepared in Example 1-3 was cut into thin slices with a thickness of 1 mm using a multi-wire saw, and then washed in alcohol and gasoline, and then ultrasonically cleaned, taken out and dried, and ground in an agate mortar with a garnet structure with alcohol added. The particle size was required to be less than 200 mesh. The crystal structure was tested using a Bruker D8 QUEST X-ray diffractometer, with a radiation source of CuKα line with a wavelength of λ=0.154 nm, a tube voltage of 40 kV, a tube current of 450 mA, a minimum step of 0.0001, a graphite monochromator, and a laboratory temperature of 24°C. The XRD pattern was shown in FIG. Figure 1 .
[0081] pass Figure 1 It can be seen from the XRD images that the distribution and relative intensity of the diffraction peaks of the quartz crystals prepared in Examples 1-3 are consistent with the standard quartz cards, which proves that the microstructure of the quartz crystals grown in each embodiment of the present invention is relatively ideal, and the products prepared in each embodiment of the present invention are all quartz crystals.
[0082] The Q value of crystal is the macroscopic manifestation of the microscopic defects in its internal structure. The infrared absorption coefficient α is measured by Shimadzu Tracer-100 Fourier transform infrared spectrometer, and the Q value is calculated by the following relationship:
[0083]
[0084] Where D is the sample thickness (cm), T1 is the band baseline 3900cm -1 T2 is the transmittance of the absorption band, and the Q value results are shown in Figure 2 .
[0085] Depend on Figure 2 It can be seen that the piezoelectric crystals prepared in various embodiments of the present invention have lower Q values, indicating that the present invention uses a silicon-containing Gemini surfactant together with a hydrochloric acid solution to effectively reduce impurities in the quartz stone, thereby reducing defects inside the crystal, and the obtained crystal has higher quality.
[0086] The surface of the crystal of each embodiment and comparative example was scanned using a Brolight SEK-8501 scanning tunneling microscope to obtain a high-resolution image of the corrosion tunnel. The number of corrosion tunnels per unit area was counted using image analysis software, thereby calculating the density of the corrosion tunnel. The results are shown in Figure 3 .
[0087] Depend on Figure 3 It can be seen that the corrosion tunnel density of the piezoelectric crystals prepared in each embodiment of the present invention is lower, indicating that the piezoelectric performance and reliability of the prepared piezoelectric crystals are higher, indicating that the performance of the piezoelectric crystals can be effectively improved by the method of the present invention, and high-quality piezoelectric crystals can be obtained.
[0088] The total impurity content of the piezoelectric crystals prepared in each embodiment and comparative example was measured using an ICP-MS2000 series inductively coupled plasma mass spectrometer. The results are shown in Figure 4 .
[0089] Depend on Figure 4 It can be seen that the piezoelectric crystal obtained by the growth method of the present invention has a lower impurity content and a purity level of 4N5 (SiO2=99.995%) or above, which shows that the present invention uses a silicon-containing Gemini-type surfactant and a hydrochloric acid solution together to obtain a piezoelectric crystal with high quality and high purity. In addition, the time for obtaining the piezoelectric crystal by heat preservation and pressure preservation in each embodiment of the present invention is shorter than that in the comparative example, which proves that the present invention shortens the production cycle and can obtain piezoelectric crystal more quickly.
[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0091] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A method for rapidly growing high-quality and high-purity piezoelectric crystal, characterized in that: The steps include: S1. Mix terminal allyl polyether and diglycolic anhydride, introduce nitrogen, heat to 50-60° C., add hydroxypropyl-terminated polydimethylsiloxane and tricyclohexylphosphine, stir evenly, and finally add diallyl isocyanurate and palladium acetate to obtain a silicon-containing Gemini surfactant; S2, after natural quartz stone is sorted, it is washed with deionized water to remove surface impurities, and then the sorted natural quartz stone is placed in a trough, the trough is immersed in a hydrochloric acid solution, and then the silicon-containing Gemini surfactant is added, and the hydrochloric acid solution is ultrasonically treated by an ultrasonic device. After 10-20 minutes, the trough is taken out, and the trough is quickly immersed in deionized water at room temperature for rapid cooling, and the ultrasonic and rapid cooling process is repeated again. The obtained quartz material is crushed and sieved, and the quartz crushed material with a diameter of 1.5-3cm is selected as the culture body, and is placed in the lower part of the autoclave; S3, high-purity water is loaded into the autoclave, the piezoelectric crystal is cut along the c direction to obtain the Z-axis seed crystal, the Z-axis seed crystal is placed in a hydrofluoric acid solution and soaked for 4-5 hours, then washed with deionized water, and then cut and punched, the seed crystal is hung on a seed crystal rack, and then the seed crystal rack is loaded into the autoclave, an isolation plate is set on the seed crystal rack, and convection holes are set on the isolation plate, and then the autoclave is sealed; S4, start the autoclave, perform programmed temperature control on the upper and lower parts of the autoclave respectively, and obtain the piezoelectric crystal after maintaining the temperature and pressure for 50-55 days.
2. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 1, characterized in that: The feeding mass ratio of the terminal allyl polyether, diglycolic anhydride, hydroxypropyl-terminated polydimethylsiloxane, tricyclohexylphosphine, diallyl isocyanurate and palladium acetate is 80-120:10-15:120-150:1-5:20-30:1-5.
3. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 2, characterized in that: The mass fraction of the hydrochloric acid solution is 10%-20%.
4. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 3, characterized in that: The amount of the silicon-containing Gemini surfactant used is 1%-5% of the mass of the hydrochloric acid solution.
5. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 4, characterized in that: The power of the ultrasonic treatment is 20-35 W / L, and the temperature is 60-80°C.
6. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 5, characterized in that: The mass fraction of the hydrofluoric acid solution is 20%-30%.
7. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 6, characterized in that: The filling degree of the high-purity water is 75%-85%.
8. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 7, characterized in that: The diameter of the convection holes on the isolation plate is 15-30 mm, and the opening rate of the isolation plate is 4%-8%.
9. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 8, characterized in that: The pressure of the autoclave is 140-160 MPa.
10. The method for rapidly growing high-quality and high-purity piezoelectric crystal according to claim 9, characterized in that: The upper part of the autoclave is heated to 100-110°C at 4°C / min, kept at this temperature for 4 hours, then heated to 230-250°C at 4°C / min, kept at this temperature for 20 hours, and then heated to 320-340°C at 4°C / min, and kept at this temperature until the growth is completed; The upper part of the autoclave is heated to 120-130°C at 4°C / min, kept warm for 4 hours, then heated to 260-270°C at 4°C / min, kept warm for 20 hours, and then heated to 340-360°C at 4°C / min, and kept warm until the growth is completed.