Method for preparing gypsum whiskers from high-calcium gasification slag

By adding sulfuric acid to the coal gasified slag acid solution to regulate the reaction conditions, the problem of high calcium content in the coal gasified slag affecting the quality of PAC products was solved, and gypsum whiskers with different aspect ratios were prepared, which improved product quality and resource utilization efficiency. , meets a variety of application needs.

CN118910737APending Publication Date: 2024-11-08KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410840610.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When the calcium content in coal gasification slag is high, it is difficult to meet the requirements of GB/T22627 standards, which affects the quality of the product. There is no report on the preparation of gypsum whiskers using coal gasification slag acid solution in the prior art.

Method used

By adding sulfuric acid dropwise to regulate the reaction conditions in the acid solution, the removal of calcium is achieved, and the gypsum whiskers with different aspect ratios are prepared to meet different length and diameter ratios by taking advantage of the low solubility of gypsum. The application market demand is achieved, while the acid solution is decalcified and aluminum-rich, creating conditions for the preparation of PAC flocculants.

Benefits of technology

It improves the quality and added value of PAC flocculants, enhances the economy of resource utilization of coal gasification slag, and realizes the efficient preparation of gypsum whiskers to meet different market demands.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure BDA0004914288390000081
    Figure BDA0004914288390000081
Patent Text Reader

Abstract

The invention relates to a method for preparing gypsum whiskers from high-calcium gasified slag. A gasified slag acid solution is obtained by extracting an acid-soluble substance from the gasified slag through hydrochloric acid. As the calcium content is high, and the product quality is seriously influenced during the subsequent preparation of the aluminum chloride flocculant, the decalcification is carried out in a gypsum whisker production mode by virtue of a sulfuric acid decalcification process, so that the added value of the decalcified product is increased while the quality of the flocculant product is improved, and the method has very important significance on improving the overall economical efficiency of resource utilization of the gasified slag. According to the method, the gasified slag acid solution and the primary washing liquid are used as raw materials, the average length-diameter ratio of the gypsum whiskers prepared from the acid solution is 10-80 by regulating and controlling the technological parameters such as the concentration of sulfuric acid, the dripping speed, the temperature and the aging time, and the average length-diameter ratio of the gypsum whiskers prepared from the gasified slag primary washing liquid is 150-200; and the composite material can be used as a reinforcing agent or functional filler in resin, rubber, coating and papermaking, can also be used for friction materials, building materials, sealing materials, heat-insulating and flame-retardant materials and the like, and has an extremely wide development prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of waste liquid recycling and safe disposal, relates to the recovery and harmless treatment of valuable elements in industrial solid waste, and specifically relates to a method for preparing gypsum whiskers from high-calcium gasified slag. Background Art

[0002] Coal gasification slag is one of the by-products of the coal gasification process and is classified as industrial solid waste. At present, coal gasification slag is mainly stored in piles, which occupies a large amount of land space and has the risk of land and water pollution. Therefore, the development of coal gasification slag resource utilization technology is imminent.

[0003] Gasification slag is a high-temperature water-quenched product. Generally, the inorganic minerals in the ash are mainly silicon and aluminum, with high residual carbon content, large specific surface area, and good reactivity and volcanic ash activity. At present, the resource utilization of coal gasification slag at home and abroad can be roughly divided into four aspects, mainly including: ① Building materials, such as the preparation of ceramsite, cement, concrete, unburned bricks, wall materials, etc., which is the most direct way to consume gasification slag on a large scale; ② Utilization of residual carbon, such as carbon extraction and quality separation, cyclic blending, adsorption materials, etc.; ③ Soil improvement materials, such as soil improvement, water body restoration, ecological fertilizer, etc.; ④ High-value utilization, such as catalyst carriers, porous materials, aluminum-based materials, silicon-based materials, etc. Because my country's energy structure lacks oil and is rich in coal, coal gasification has become the main development mode of deep coal processing and the mainstream direction of coal chemical industry. In the future, coal gasification slag will increase exponentially. With the increase in the output of coal gasification slag, the pressure on its resource utilization has doubled. Faced with the additional output of tens of millions of tons each year, it is necessary to combine it with local actual conditions and use multiple approaches to achieve its resource utilization.

[0004] Since coal gasification slag has good reactivity, in recent years, using coal gasification slag to extract valuable elements to produce chemical products and improve the resource utilization value of coal gasification slag has become a research hotspot. Li Yanhuan et al. reported in the article "Experimental Study on Preparation of Polyaluminium Chloride from Coal Gasification Slag by Removing Impurities and Enriching Aluminium" that polyaluminium chloride products that meet the quality of GB / T 22627 were prepared using gasification slag acid solution; Wu Qin et al. used coal gasification acid slag to wet silicon extraction to produce water glass, while increasing the alkali residue carbon content to facilitate the subsequent preparation of high value-added activated carbon; Xiong et al. used enhanced mass transfer hydrothermal method to extract Al from coal gasification slag in one acid solution. 3+ , polyaluminum chloride prepared by alkalization and polymerization of calcium aluminate powder; He et al. used coal gasification slag as raw material and prepared multi-ion composite flocculant by one-step acid dissolution method, and applied it to the treatment of kaolin simulated wastewater; Pan et al. used coal gasification crude slag as raw material and adopted hydrochloric acid and acetic acid two-step acid dissolution method to prepare a new type of polyaluminum-acetic acid-ferric chloride flocculant composite flocculant (PAFAC).

[0005] In summary, one of the main ways to utilize coal gasification slag in high value is to extract aluminum by acid dissolution, extract silicon by alkali dissolution and enrich carbon in alkali residue. Aluminum products are mainly used to produce PAC flocculants, but when the calcium content in coal gasification slag is high, the produced PAC is difficult to meet the requirements of GB / T22627 standard, especially when producing solid products, which seriously affects the aluminum content in the product. Therefore, acid solution decalcification has become an important measure to ensure the quality of PAC flocculants prepared from coal gasification slag.

[0006] When coal gasification slag is used to prepare PAC, its acid-soluble products exist in the acid solution in the form of hydrochloride. At this time, when sulfuric acid is added to the acid solution, calcium will be converted into insoluble calcium sulfate dihydrate, thereby achieving calcium removal. When the reaction conditions are optimized and controlled, gypsum whiskers can be obtained while decalcifying.

[0007] Gypsum whisker is a fiber sub-nano material that combines the advantages of both reinforcing fiber and ultrafine inorganic filler. It is specifically divided into dihydrate calcium sulfate whisker, hemihydrate calcium sulfate whisker and anhydrous calcium sulfate whisker. They all have excellent physical and chemical properties such as high strength, high modulus, high toughness, high insulation, chemical corrosion resistance, and easy to composite with polymers. Due to its excellent performance and excellent performance-price ratio, it has a wide range of applications and broad market prospects. At present, the preparation of gypsum whiskers is mainly based on recrystallization, such as the use of chemical byproduct phosphogypsum hydrothermal method to prepare gypsum whiskers, and the use of chemical precipitation method is relatively rare: Ma Yuanyuan et al. reported in the article "Study on the process of preparing hemihydrate calcium sulfate whiskers from calcium chloride" that calcium chloride and sodium sulfate were used as the main raw materials, concentrated hydrochloric acid was used to adjust the pH, different crystal growth promoters were selected, and hemihydrate calcium sulfate whiskers were prepared by atmospheric pressure acidification. Its aspect ratio reaches 50; Zhu Yudi et al. reported in the article "Study on the process of preparing calcium sulfate whiskers using sodium sulfate", the process of synthesizing dihydrate calcium sulfate precursor using sodium sulfate and calcium chloride as raw materials, and further using hydrothermal method to prepare hemihydrate calcium sulfate whiskers. The hydrothermal reaction temperature of 150℃, reaction time of 4h, solid content of 5% and initial pH=3 were determined as the optimal process conditions, and the average aspect ratio of the prepared hemihydrate calcium sulfate whiskers can reach 50-60; Wang Shouwu et al. reported in the article "Study on the preparation of high-quality dihydrate calcium sulfate whiskers from chemical wastewater", calcium sulfate prepared from chemical wastewater containing sulfate ions and calcium salt was used as raw materials, sodium hexadecyl sulfate was used as a dispersant, magnesium chloride was used as a crystal growth promoter, and sulfuric acid was used to adjust the pH, and dihydrate calcium sulfate whiskers were prepared by hydrothermal method. When the optimal reaction temperature is 125℃ and the reaction cooling rate is 30℃ / 30min, the aspect ratio can reach more than 80.

[0008] In summary, there is no report on the use of coal gasification slag acid solution to prepare gypsum whiskers. Therefore, the present invention utilizes the low solubility of dihydrate gypsum, combined with the difference in calcium ion concentration between the acid solution and the first washing liquid, to prepare gypsum whiskers with different aspect ratios by adding sulfuric acid and adjusting the reaction conditions, thereby meeting the needs of different application markets and achieving decalcification and aluminum enrichment of the acid solution, creating conditions for the preparation of PAC flocculants. Summary of the invention

[0009] When using coal gasification slag for multi-element extraction, acid dissolution is usually used to extract aluminum, and alkali dissolution is used to extract silicon and then enrich residual carbon. When the aluminum product is a PAC flocculant, calcium is almost completely transferred to the liquid phase during acid dissolution, which seriously affects the quality of subsequent PAC products. Therefore, decalcification is a necessary measure. The present invention aims at the high calcium content of high-calcium coal gasification slag, utilizes the low solubility of dihydrate gypsum, and converts the calcium ions in the acid solution into dihydrate gypsum by dripping sulfuric acid. After the reaction is completed, the temperature is naturally lowered and aged, and then the acid solution is decalcified by filtering and separation. In order to increase the added value of the decalcified product, the present invention optimizes and controls the decalcification process parameters, combines the difference in calcium ion concentration between the acid solution and the first washing liquid, and utilizes the longitudinal growth characteristics of gypsum whiskers by using aluminum and magnesium ions in the acid solution to prepare gypsum whiskers with different aspect ratios, or further dehydrates to prepare anhydrous gypsum whiskers to meet different market needs.

[0010] The present invention is achieved through the following technical solutions:

[0011] A method for preparing gypsum whiskers from high-calcium gasified slag comprises the following steps:

[0012] (1) Acid dissolution, after drying and grinding the high-calcium gasification slag, acid dissolution reaction is carried out with hydrochloric acid at a liquid-to-solid ratio of 3-4:1 under theoretical acid dosage, filtering after the reaction is completed to obtain a filter cake and an acid solution, and washing the filter cake to obtain a washing liquid; the high-calcium gasification slag refers to the gasification slag produced during the coal gasification process, the calcium oxide content of which is ≥10wt%, and the remaining components are mainly silicon oxide and aluminum oxide.

[0013] (2) calcium precipitation, at a temperature of 60-80° C., adding sulfuric acid with a concentration of 0.33-3.03 mol / L to the acid solution and the first washing liquid respectively, and controlling the dropping speed to 400-800 μL / min, after the dropping is completed, the calcium ions in the acid solution and the first washing liquid are converted into dihydrate gypsum with low solubility;

[0014] (3) aging, aging the obtained dihydrate gypsum at room temperature for 12-24 hours; after the aging is completed, the aged dihydrate gypsum is obtained;

[0015] (4) decalcification, filtering and washing the aged dihydrate gypsum to obtain dihydrate gypsum whiskers and a decalcification solution;

[0016] (5) Dehydration: further dehydrating the obtained dihydrate gypsum whiskers to obtain anhydrous gypsum whiskers.

[0017] The dihydrate gypsum whiskers prepared from the acid solution in step (4) have an aspect ratio of 10-80 and a length of 50-200 μm; the dihydrate gypsum whiskers prepared from a wash solution have an aspect ratio of 150-200 and a length of 1800-2500 μm.

[0018] The concentration of the hydrochloric acid in step (1) is 32-35%.

[0019] The process of washing the filter cake in step (1) is a cyclic washing process, which is as follows: the filter cake is washed for the first time using process water and / or a second washing liquid, and the liquid after washing is a first washing liquid; the filter cake after the first washing is washed for the second time using process water and / or a third washing liquid, and the liquid after washing is a second washing liquid; the filter cake after the second washing is washed for the third time using process water, and the liquid after washing is a third washing liquid. During the first washing, process water is used for the first washing, the second washing and the third washing, and the liquids after washing are a first washing liquid, a second washing liquid and a third washing liquid, respectively. During the subsequent washing process, the second washing liquid replaces the process water of the first washing, and the third washing liquid replaces the process water of the second washing. If the second washing liquid and the third washing liquid are not enough to complete the washing, some process water is supplemented.

[0020] The decalcified liquid obtained in step (4) is divided into two types, namely, the decalcified liquid obtained from the first washing liquid and the decalcified liquid obtained from the acid solution; the decalcified liquid obtained from the first washing liquid is returned to step (1) for acid dissolution with hydrochloric acid; the decalcified liquid obtained from the acid solution is used to prepare the flocculant product.

[0021] The technical principles of the present invention are as follows:

[0022] Coal gasification slag is a high-temperature water-quenched product. Its inorganic minerals mainly exist in the form of glass and have good reaction activity. When hydrochloric acid is used as the reaction medium, the aluminum, calcium, iron, and magnesium elements therein combine with chloride ions to form soluble substances and transfer into the liquid phase. After filtration and washing, acid solution and a washing liquid can be obtained. Since the amount of residual carbon in the coal gasification slag is relatively high and has good adsorption, the soluble salt content in the washing liquid is high. When used as a subsequent reaction liquid, it will seriously affect the dissolution effect of soluble elements in the coal gasification slag. After decalcification, not only the amount of hydrochloric acid used can be reduced, but also the dissolution effect can be improved.

[0023] When sulfuric acid is added to the gasification slag acid solution or the first washing liquid, calcium ions will quickly combine with sulfate to produce calcium sulfate. As the amount of sulfuric acid added increases, calcium sulfate is in a supersaturated state and then forms solidified calcium sulfate. Because the reaction is carried out in the liquid phase and the temperature is low, calcium sulfate crystals are further transformed into dihydrate calcium sulfate with lower solubility. At the same time, there are a large number of aluminum, magnesium and other ions in the acid solution, which provide conditions for the longitudinal growth of dihydrate gypsum. In order to reduce the breakage rate of whiskers, the decalcification process does not require stirring. Only by extending the aging time of the reaction system, the chemical reaction is completed by ion diffusion, which not only reduces power consumption, but also reduces mechanical damage caused by stirring. After the acid is added, the temperature drops naturally, reducing the solubility of calcium sulfate and promoting the formation of dihydrate gypsum. At the same time, by extending the aging time, it is helpful for calcium ions and sulfate ions to fully contact and transform, and reduce the calcium ion concentration of the decalcification system. After aging, the difference in the growth rate of gypsum on different crystal faces is used to further increase the aspect ratio of gypsum whiskers. On the other hand, due to the large difference in ion concentration between the acid solution and the first washing liquid, the growth behavior of gypsum crystals will be seriously affected, resulting in a difference in the aspect ratio of gypsum whiskers prepared by the acid solution and the first washing liquid. According to different market needs, the above dihydrate gypsum whiskers are dehydrated to obtain anhydrous gypsum whiskers.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The extraction of multiple elements from coal gasification slag is one of the important means for high-value utilization of coal gasification slag. Currently, the most common method is to use hydrochloric acid to extract the acid-soluble material to prepare PAC flocculant, and to use the acid slag plus alkali wet method to prepare water glass to recover silicon and further enrich carbon, thereby creating conditions for preparing activated carbon from alkaline slag. However, the calcium content in the gasification slag is relatively high, which will seriously affect the quality of aluminum products. The acid-soluble decalcification technical means of the present invention can well make up for the above-mentioned defects.

[0026] The components in the hydrochloric acid reaction liquid of coal gasification slag are hydrochloride, that is, calcium ions exist in the form of calcium chloride. The solubility of calcium chloride at room temperature is as high as 75%, while that of calcium sulfate dihydrate is only about 0.2%. At the same time, sulfuric acid is a conventional industrial product with low value, so it is effective to remove calcium from the acid solution of gasification slag by dripping sulfuric acid. The present invention achieves the purpose of decalcification by generating gypsum whiskers through the control of sulfuric acid decalcification process parameters. While improving the quality of flocculant products, it increases the added value of decalcified products, which is of great significance to the overall economic efficiency of gasification slag resource utilization. At the same time, the method of the present invention has the characteristics of simple process, wide applicable range of acid solution concentration, and high added value of products, which can better improve the economic efficiency of multi-element extraction of coal gasification slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a process flow chart of the present invention;

[0028] Figure 2This is a process flow chart of the washing step in step (1) of the present invention. DETAILED DESCRIPTION

[0029] In order to further illustrate the decalcification of coal gasification slag acid solution, the main hydrochloric acid salt compositions of gasification slag acid solutions with different liquid-to-solid ratios and a washing solution are listed as follows:

[0030] Table 1 Chemical composition analysis results of gasification slag acid solution (wt%)

[0031] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 8.40-11.20 2.29-3.05 0.33-0.43 2.45-3.25 6.54-8.72 0.60-0.80 0.60-0.80

[0032] Table 2 Chemical composition analysis results of gasification slag-washing liquid (wt%)

[0033] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 1.18-1.57 0.48-0.64 0.12-0.16 0.55-0.74 0.95-1.27 0.13-0.17 0.13-0.17

[0034] Take a certain mass of acid solution or a washing liquid, calculate the amount of sulfuric acid to be added according to the chemical composition analysis results of the decalcified liquid, and then prepare a sulfuric acid solution of a certain concentration, use a peristaltic pump to add sulfuric acid at a certain drop rate, and after the acid addition is completed, naturally cool down and age for a certain period of time, then filter, wash and dry to obtain dihydrate gypsum whiskers, and the dihydrate gypsum whiskers are further dehydrated to obtain anhydrous gypsum.

[0035] The active ingredient that reacts chemically with hydrochloric acid is mainly CaCl2. The chemical equation of the reaction is shown in formula (1):

[0036] CaCl2+H2SO4→CaSO4+2HCl(1)

[0037] According to formula (1), the theoretical acid consumption required for pickling solution is calculated as follows:

[0038]

[0039] In the formula: m is the theoretical consumption mass of H2SO4, g; ωi is the mass fraction of metal chloride i in Table 1 or Table 2, %; Mi is the relative molecular mass of metal chloride i in Table 1 or Table 2, g / mol; λi is the valence of metal element i in Table 1 or Table 2; Pi is the number of metal atoms in metal chloride i in Table 1 or Table 2, g / mol; MH2SO4 is the relative molecular mass of sulfuric acid, g / mol; ωH2SO4 is the mass fraction of sulfuric acid solution, %.

[0040] It is calculated by formula (2) that when decalcification is performed with an acid solution, the theoretical acid consumption for CaCl2 precipitation is 11.14-14.86 g (96.5% sulfuric acid); when decalcification is performed with a wash solution, the theoretical acid consumption for CaCl2 precipitation is 1.62-2.16 g (96.5% sulfuric acid).

[0041] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited by the embodiments.

[0042] Example 1

[0043] Take a certain mass of acid solution, its main chemical composition is shown in Table 1-1:

[0044] Table 1-1 Chemical composition analysis results of the gasified slag acid solution used in Example 1 (wt%)

[0045] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 11.20 3.05 0.43 3.25 8.72 0.80 0.80

[0046] The above acid solution was placed in a water bath at 80°C. After theoretical calculation, diluted sulfuric acid with a concentration of 3.03 mol / L was prepared according to the theoretical acid dosage. The solution was continuously added dropwise at a rate of 600 μL / min using a peristaltic pump. After the addition, the solution was naturally cooled to room temperature and aged for 12 hours. Calcium sulfate dihydrate whiskers were obtained after filtration and washing. Further dehydration gave anhydrous gypsum whiskers. The relevant performance indicators are shown in Table 1-2.

[0047] Table 1-2 Related properties of anhydrous gypsum whiskers obtained in Example 1

[0048]

[0049] Example 2

[0050] Take a certain mass of acid solution, its main chemical composition is shown in Table 2-1:

[0051] Table 2-1 Chemical composition analysis results of the gasified slag acid solution used in Example 2 (wt%)

[0052] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 9.74 2.80 0.39 2.80 7.73 0.60 0.60

[0053] The above acid solution was placed in a 70°C water bath. After theoretical calculation, it was prepared into dilute sulfuric acid with a concentration of 2.65 mol / L according to the theoretical acid dosage. It was continuously added dropwise with a peristaltic pump at a dropping speed of 400 μL / min. After the addition was completed, it was naturally cooled to room temperature and aged for 18 hours. After filtering and washing, dihydrate calcium sulfate whiskers were obtained, and further dehydration was performed to obtain anhydrous gypsum whiskers. Its relevant performance indicators are shown in Table 2-2.

[0054] Table 2-2 Related properties of anhydrous gypsum whiskers obtained in Example 2

[0055]

[0056] Example 3

[0057] Take a certain mass of acid solution, its main chemical composition is shown in Table 3-1:

[0058] Table 3-1 Chemical composition analysis results of the gasified slag acid solution used in Example 3 (wt%)

[0059] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 8.40 2.29 0.33 2.45 6.54 0.60 0.60

[0060] The above acid solution was placed in a 60°C water bath. After theoretical calculation, it was prepared into dilute sulfuric acid with a concentration of 2.27 mol / L according to the theoretical acid dosage. It was continuously added dropwise with a peristaltic pump at a dropping speed of 800 μL / min. After the addition was completed, it was naturally cooled to room temperature and aged for 24 hours. After filtering and washing, dihydrate calcium sulfate whiskers were obtained. Further dehydration gave anhydrous gypsum whiskers. Its relevant performance indicators are shown in Table 3-2.

[0061] Table 3-2 Related properties of anhydrous gypsum whiskers obtained in Example 3

[0062]

[0063] Example 4

[0064] Take a certain mass of a wash solution, its main chemical composition is shown in Table 4-1:

[0065] Table 4-1 Chemical composition analysis results of the washing liquid used in Example 4 (wt%)

[0066] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 1.57 0.64 0.16 0.74 1.27 0.13 0.13

[0067] The above-mentioned washing liquid was placed in a water bath at 80°C, and 0.39 mol / L sulfuric acid was continuously added by a peristaltic pump at a drop rate of 600 μL / min. After the addition was completed, the temperature was naturally cooled to room temperature and aged for 18 hours. After filtering and washing, dihydrate calcium sulfate whiskers were obtained. Its relevant performance indicators are shown in Table 4-2.

[0068] Table 4-2 Related properties of anhydrous gypsum whiskers obtained in Example 4

[0069]

[0070] Example 5

[0071] Take a certain mass of a wash solution, its main chemical composition is shown in Table 5-1:

[0072] Table 5-1 Chemical composition analysis results of the washing liquid used in Example 5 (wt%)

[0073] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 1.36 0.55 0.14 0.67 1.09 0.14 0.13

[0074] The above-mentioned washing liquid was placed in a 60°C water bath, and 0.33 mol / L sulfuric acid was continuously added at a drop rate of 800 μL / min using a peristaltic pump. After the addition, the temperature was naturally cooled to room temperature and aged for 24 hours. After filtering and washing, dihydrate calcium sulfate whiskers were obtained. The relevant performance indicators are shown in Table 5-2.

[0075] Table 5-2 Related properties of anhydrous gypsum whiskers obtained in Example 5

[0076]

[0077] Example 6

[0078] Take a certain mass of a wash solution, its main chemical composition is shown in Table 6-1:

[0079] Table 6-1 Chemical composition analysis results of the washing liquid used in Example 6 (wt%)

[0080] <![CDATA[AlCl3]]> <![CDATA[FeCl2]]> <![CDATA[FeCl3]]> <![CDATA[MgCl2]]> <![CDATA[CaCl2]]> KCl NaCl 1.18 0.48 0.12 0.55 0.95 0.17 0.17

[0081] The above-mentioned washing liquid was placed in a 70°C water bath, and 0.44 mol / L sulfuric acid was continuously added by a peristaltic pump at a drop rate of 400 μL / min. After the addition, the temperature was naturally lowered to room temperature and aged for 12 hours. After filtering and washing, dihydrate calcium sulfate whiskers were obtained. The relevant performance indicators are shown in Table 6-2.

[0082] Table 6-2 Related properties of anhydrous gypsum whiskers obtained in Example 6

[0083]

[0084] It can be seen from Examples 1-6 that the average aspect ratio of the anhydrous gypsum whiskers prepared by acid solution is 10-80, and the average aspect ratio of the anhydrous gypsum whiskers prepared by gasified slag-washing liquid is 150-200. They can be used as reinforcing agents or functional fillers in resins, rubbers, coatings, and papermaking, and can also be used in friction materials, building materials, sealing materials, thermal insulation and flame retardant materials, etc., and have extremely broad development prospects.

Claims

1. A method for preparing gypsum whiskers from high-calcium gasified slag, It is characterized in that The following steps are included: (1) Acid dissolution: After drying and grinding the high-calcium fumed slag, acid dissolution reaction is carried out with hydrochloric acid at a liquid-to-solid ratio of 3-4:1 under the theoretical acid dosage of the high-calcium fumed slag. After the reaction is completed, filter to obtain a filter cake and an acid solution, and wash the filter cake to obtain a washing liquid; (2) Calcium precipitation: at a temperature of 60-80°C, sulfuric acid with a concentration of 0.33-3.03 mol / L is added to the acid solution and the first washing liquid respectively, and the dropping speed is controlled to be 400-800 μL / min. After the dropping is completed, the calcium ions in the acid solution and the first washing liquid are converted into dihydrate gypsum with low solubility; (3) Aging, aging the obtained dihydrate gypsum at room temperature for 12-24 hours; after the aging, the aged dihydrate gypsum is obtained; (4) decalcification, filtering and washing the aged dihydrate gypsum to obtain dihydrate gypsum whiskers and decalcification liquid; (5) Dehydration: further dehydrating the obtained dihydrate gypsum whiskers to obtain anhydrous gypsum whiskers.

2. A method for preparing gypsum whiskers from high-calcium gasified slag according to claim 1, It is characterized in that The aspect ratio of the dihydrate gypsum whiskers prepared from the acid solution in step (4) is 10-80, and the length is 50-200 μm; the aspect ratio of the dihydrate gypsum whiskers prepared from a washing solution is 150-200, and the length is 1800-2500 μm.

3. The method for preparing gypsum whiskers from high-calcium gasified slag according to claim 1, It is characterized in that The concentration of the hydrochloric acid in step (1) is 32-35%.

4. The method for preparing gypsum whiskers from high-calcium gasified slag according to claim 1, It is characterized in that The process of washing the filter cake in step (1) is as follows: using process water and / or a second washing liquid to wash the filter cake for the first time, and the liquid after washing is the first washing liquid; using process water and / or a third washing liquid to wash the filter cake after the first washing for the second time, and the liquid after washing is the second washing liquid; The filter cake after the second washing is washed for the third time with process water, and the liquid after washing is the third washing liquid.

5. The method for preparing gypsum whiskers from high-calcium gasified slag according to claim 1, It is characterized in that The decalcified liquid obtained in step (4) is divided into two types, namely, the decalcified liquid obtained from the first washing liquid and the decalcified liquid obtained from the acid solution; the decalcified liquid obtained from the first washing liquid is returned to step (1) for acid dissolution with hydrochloric acid; the decalcified liquid obtained from the acid solution is used to prepare the flocculant product.

6. The method for preparing gypsum whiskers from high-calcium gasified slag according to claim 1, It is characterized in that The high-calcium gasification slag refers to the coal gasification slag produced during the coal gasification process, in which the calcium oxide content is ≥10wt%, and the remaining components are mainly silicon oxide and aluminum oxide.