Environment-friendly polyester bath durable flame retardant and preparation method thereof
By using N-dimethoxyphosphorylpropionylphthalimide and surfactant in a polyester bath, a durable flame retardant in an environmentally friendly polyester bath was prepared, which solved the existing polyester durability resistance. The inability of the combustion agent to be treated in the bath is unfriendly and the environmentally friendly problem is achieved, achieving efficient and environmentally friendly flame retardant performance and wash resistance.
Patent Information
- Application Number
- CN202411107116.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
AI Technical Summary
The existing polyester durable flame retardants cannot be treated in the bath, which limits the processing conditions of polyester materials. In addition, the flame retardants in the polyester baths on the market contain halogen, which is harmful to the environment.
Using a combination of N-dimethoxyphosphorylpropionylphthalimide, anionic surfactant and nonionic surfactant, the environmentally friendly polyester bath is prepared by heating and insulation treatment, suitable for polyester Durable flame retardant finish for yarns and velvets.
It realizes a durable flame retardant in a halogen-free polyester bath with low cost and superior flame retardant performance. It is suitable for the durable flame retardant finish of polyester in various structures, and has good washing resistance, completely replacing the flame retardant performance of commercially available products and Wash resistance.
Smart Images

Figure CN118910883A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of functional finishing agents for textiles, and in particular to an environmentally friendly polyester bath durable flame retardant and a preparation method thereof. Background Art
[0002] The so-called flame retardant finishing means that after the flame retardant treatment, the flammability of the textile is reduced, the burning rate can be significantly slowed down during the combustion process, and it will quickly self-extinguish after leaving the fire source, thus having the property of being non-flammable; durable flame retardant finishing means that after 30 to 50 ordinary household machine washes after flame retardant finishing, the flame retardant finishing can still meet the flame retardant standards.
[0003] Polyester fabrics have the advantages of high strength, wear resistance, good resilience, and low cost, and are widely used as textile fabrics. However, the limiting oxygen index (LOI) of polyester fiber is relatively low, only about 20, and it is a flammable fiber, so flame retardant finishing is required. The flame retardants for polyester fabrics are mostly halogen and phosphorus flame retardants. Halogen flame retardants release hydrogen halides during combustion, which are toxic and corrosive, so halogen flame retardants are not environmentally friendly; phosphorus flame retardants have a good flame retardant effect on polyester fibers containing carbon and oxygen elements. At high temperatures, phosphorus catalyzes the carbonization of polymers, reduces the generation of combustible gases, and isolates the air, and achieves flame retardancy through condensation.
[0004] The polyester durable flame retardants currently on the market are cyclic phosphonates (domestic patent number: 101608401A). This type of polyester durable flame retardant can only be processed in a setting machine through dipping, drying and baking. Some polyester materials such as yarn and loose fiber cannot be used on the setting machine, thus limiting the processing conditions of polyester materials. The polyester bath flame retardants on the market, such as hexabromocyclododecane, decabromodiphenylethane and other flame retardant dispersions, contain halogens themselves and will release hydrogen halide gas during combustion, which is toxic and corrosive, harmful to the human body and the environment, and not environmentally friendly.
[0005] Therefore, an environmentally friendly polyester bath durable flame retardant with simple preparation process, halogen-free, easy to use and a preparation method thereof are in urgent need of emergence. Summary of the invention
[0006] The purpose of the present application is to provide an environmentally friendly polyester bath durable flame retardant and a preparation method thereof, so as to solve the technical problems that the existing polyester durable flame retardant cyclic phosphate ester cannot be processed in a bath and can only be processed by padding, drying and baking, which limits the processing conditions of polyester materials; and the existing polyester bath durable flame retardant is not environmentally friendly.
[0007] The present application provides an environmentally friendly polyester bath durable flame retardant, the general structural formula of which is:
[0008]
[0009] The invention comprises the following raw materials in parts by weight: 75%-85% of N-dimethoxyphosphorylpropionylphthalimide, 5%-15% of anionic surfactant and 5%-20% of nonionic surfactant.
[0010] Preferably, the anionic surfactant includes one or more of dodecylbenzene sulfonic acid, sulfonated NongRu 600#, and sulfonated NongRu 600#F; the nonionic surfactant includes one or more of NongRu 600#, fatty alcohol polyoxyethylene ether AEO-9, and fatty alcohol polyoxyethylene ether AEO-10.
[0011] The present application provides a method for preparing the above-mentioned environmentally friendly durable flame retardant in polyester bath: N-dimethoxyphosphorylpropionylphthalimide is mixed with anionic surfactants and nonionic surfactants, the temperature is raised to 50-60°C, and the temperature is kept for 20-40 minutes to obtain the environmentally friendly durable flame retardant in polyester bath.
[0012] Preferably, the preparation steps of N-dimethoxyphosphorylpropionylphthalimide are as follows:
[0013] S1: dimethyl phosphite and acrylamide are first mixed, the temperature is raised to 50-60°C, sodium methoxide is used as a catalyst, and sodium methoxide is slowly added to the mixed solution of dimethyl phosphite and acrylamide to react, and dimethoxyphosphoryl propionamide is obtained after the reaction;
[0014] S2 cools the temperature to 40-50° C., adds phthalic anhydride to the dimethoxyphosphoryl propionamide obtained in step S1, performs a ring-opening reaction, and then performs a dehydration ring-closing reaction to obtain N-dimethoxyphosphoryl propionyl phthalimide.
[0015] Preferably, in step S1, the molar ratio of dimethyl phosphite to acrylamide and sodium methoxide is 1:(1.05-1.15):(0.1-0.3).
[0016] Preferably, in step S2, the molar ratio of phthalic anhydride to dimethoxyphosphorylpropionamide is 1:(1.05-1.15).
[0017] Preferably, in step S1, when sodium methoxide is added to the mixed solution of dimethyl phosphite and acrylamide, the temperature is controlled at 71-80°C, and after the addition, the mixture is kept at 80-86°C for 3-5 hours to obtain dimethoxyphosphorylpropionamide.
[0018] Preferably, in step S2, phthalic anhydride is added to the dimethoxyphosphorylpropionamide obtained in step S1, and then the temperature is raised to 60-80° C. and kept warm for 1-3 hours to carry out a phthalic anhydride ring-opening reaction; after the reaction, the temperature is raised to 140-160° C. and a dehydration ring-closing reaction is carried out for 4-6 hours under a vacuum degree of -0.1-0.08 MPa.
[0019] The present application provides an application of the above-mentioned environmentally friendly polyester bath durable flame retardant in polyester, the durable flame retardant is used alone, or added when polyester is dyed, and treated in the same bath with disperse dyes at 125-130°C.
[0020] Therefore, the present application adopts the above-mentioned environmentally friendly polyester bath durable flame retardant and its preparation method, which has the following beneficial effects:
[0021] (1) The flame retardant of the present application does not use formaldehyde or halogen as raw materials during the synthesis process, has low cost, excellent flame retardant performance, is easy to use, and is particularly suitable for durable flame retardant finishing of polyester yarns and fleece.
[0022] (2) The flame retardant in the present application can be used alone or added when polyester is dyed and treated in the same bath as disperse dyes. The flame retardant in the present application contains flame retardant elements phosphorus and nitrogen, forming a phosphorus-nitrogen synergistic flame retardant effect, with a high content of flame retardant elements and good flame retardant properties. At the same time, the structure is similar to that of polyester dyeing carrier BIP and disperse dyes, and can be treated in a bath at 125-130°C to bond with the chimeric polyester and firmly bond inside the polyester. The polyester after flame retardant treatment has good wash resistance and is suitable for durable flame retardant finishing of polyesters of various structures, especially flame retardant treatment of polyester yarns in a bath. DETAILED DESCRIPTION
[0023] Example 1
[0024] (1) First, dimethyl phosphite and acrylamide are mixed, and the temperature is raised to 50°C. Sodium methoxide is used as a catalyst, and the sodium methoxide is slowly added to the dimethyl phosphite and acrylamide mixture. The temperature is controlled at 71-74°C during the addition process. After the addition, the temperature is kept at 80°C for 5 hours to obtain dimethoxyphosphoryl propionamide. The molar ratio of dimethyl phosphite to acrylamide is 1:1.05; the molar ratio of dimethyl phosphite to sodium methoxide is 1:0.1;
[0025] (2) cooling to 40°C, adding phthalic anhydride to the dimethoxyphosphoryl propionamide obtained in step (1), heating to 60°C, and keeping the temperature for 3 hours to carry out a phthalic anhydride ring-opening reaction; heating to 140°C, and carrying out a dehydration ring-closing reaction for 6 hours under a vacuum degree of -0.1 MPa to obtain N-dimethoxyphosphoryl propionyl phthalimide. The molar ratio of phthalic anhydride to dimethoxyphosphoryl propionamide is 1:1.05;
[0026] (3) The N-dimethoxyphosphoryl propionylphthalimide obtained in step (2) is mixed with anionic surfactants and nonionic surfactants in proportion, the temperature is raised to 50° C., and the temperature is kept for 40 minutes to obtain an environmentally friendly polyester bath durable flame retardant. The proportions of the components in the environmentally friendly polyester bath durable flame retardant are: 75% N-dimethoxyphosphoryl propionylphthalimide, 5% dodecylbenzene sulfonic acid, and 20% agricultural milk 600#.
[0027] Example 2
[0028] (1) First, dimethyl phosphite and acrylamide are mixed, and the temperature is raised to 55°C. Sodium methoxide is used as a catalyst, and sodium methoxide is slowly added to the dimethyl phosphite and acrylamide mixture. The temperature is controlled at 74-77°C during the addition process. After the addition, the temperature is kept at 83°C for 4 hours to obtain dimethoxyphosphoryl propionamide. The molar ratio of dimethyl phosphite to acrylamide is 1:1.1; the molar ratio of dimethyl phosphite to sodium methoxide is 1:0.2;
[0029] (2) Cooling to 45°C, adding phthalic anhydride to the dimethoxyphosphoryl propionamide obtained in step (1), heating to 70°C, and keeping the temperature for 2 hours to perform a phthalic anhydride ring-opening reaction; heating to 150°C, and performing a dehydration ring-closing reaction for 5 hours under a vacuum degree of -0.09 MPa to obtain N-dimethoxyphosphoryl propionyl phthalimide. The molar ratio of phthalic anhydride to dimethoxyphosphoryl propionamide is 1:1.1;
[0030] (3) The N-dimethoxyphosphoryl propionyl phthalimide obtained in step (2) is mixed with anionic surfactants and nonionic surfactants in proportion, the temperature is raised to 55° C., and the temperature is kept for 30 minutes to obtain an environmentally friendly polyester bath durable flame retardant. The proportions of the components in the environmentally friendly polyester bath durable flame retardant are: N-dimethoxyphosphoryl propionyl phthalimide 80%, sulfonated agricultural milk 600# 8%, and fatty alcohol polyoxyethylene ether AEO-9 12%.
[0031] Example 3
[0032] (1) First, dimethyl phosphite and acrylamide are mixed, and the temperature is raised to 60°C. Sodium methoxide is used as a catalyst, and sodium methoxide is slowly added to the dimethyl phosphite and acrylamide mixture. The temperature is controlled at 77-80°C during the addition process. After the addition, the temperature is kept at 86°C for 3 hours to obtain dimethoxyphosphoryl propionamide. The molar ratio of dimethyl phosphite to acrylamide is 1:1.15; the molar ratio of dimethyl phosphite to sodium methoxide is 1:0.3;
[0033] (2) Cooling to 50° C., adding phthalic anhydride to the dimethoxyphosphoryl propionamide obtained in step (1), heating to 80° C., and keeping the temperature for 1 h to perform a phthalic anhydride ring-opening reaction; heating to 160° C., and performing a dehydration ring-closing reaction for 4 h under a vacuum degree of -0.08 MPa to obtain N-dimethoxyphosphoryl propionyl phthalimide. The molar ratio of phthalic anhydride to dimethoxyphosphoryl propionamide is 1:1.15;
[0034] (3) The N-dimethoxyphosphoryl propionyl phthalimide obtained in step (2) is mixed with anionic surfactants and nonionic surfactants in proportion, the temperature is raised to 60° C., and the temperature is kept for 20 minutes to obtain an environmentally friendly polyester bath durable flame retardant. The proportions of the components in the environmentally friendly polyester bath durable flame retardant are: N-dimethoxyphosphoryl propionyl phthalimide 85%, sulfonated agricultural milk 600#F 5%, and fatty alcohol polyoxyethylene ether flat O-10 10%.
[0035] Application examples:
[0036] The environmentally friendly polyester bath durable flame retardant of the present invention has excellent flame retardant performance, can be embedded in polyester under certain temperature and time conditions, and has good washing resistance. Taking the hexabromocyclododecane polyester bath flame retardant on the market as a comparative example, the environmentally friendly polyester bath durable flame retardant prepared in the above embodiments is respectively subjected to flame retardant and washing resistance tests, and the specific experimental process and the obtained data are explained and verified below.
[0037] Application of durable flame retardant in the above polyester bath:
[0038] Fabric: Weight about 130g / m 2 Pure polyester woven fabric.
[0039] Flame retardant treatment process:
[0040] Flame retardant dosage 5% owf (relative to fabric weight)
[0041] Glacial acetic acid 0.3g / L
[0042] Bath ratio 1:20
[0043] The working solution prepared according to the above formula was put into a steel cup, and polyester woven fabric was added. The temperature was raised to 130°C at 2°C / min and kept warm for 30 minutes. The temperature was then lowered to below 50°C, washed with water, and dried.
[0044] Flame retardancy and washability test
[0045] Refer to "GB / T 5455-1997 Textiles Burning Performance Test Vertical Method" to test the damaged carbon length, afterflaming and smoldering time of polyester fabrics.
[0046] The flame retardant properties of the fabric after 30 washes were tested according to "GB / T17596-1998 Commercial Washing Procedure before Textile Fabric Burning Test".
[0047] Table 1 Combustion results
[0048]
[0049] It can be seen from the carbon length data in the above table that the flame retardant performance of the environmentally friendly durable flame retardant in polyester bath of the present invention is consistent with or better than that of commercially available hexabromocyclododecane; it can be seen from the increase in carbon length after washing that the washing resistance of the flame retardant of the present invention is also slightly better than that of commercially available hexabromocyclododecane; it means that the environmentally friendly durable flame retardant in polyester bath described in the present invention can completely replace the commercially available product, has better flame retardant performance and washing resistance, and is completely environmentally friendly.
[0050] Therefore, the present application provides an environmentally friendly polyester bath durable flame retardant and a preparation method thereof, which solves the technical problems that the existing polyester bath durable flame retardant cyclic phosphate cannot be processed in a bath and can only be processed by dipping, rolling, drying and baking, and the existing polyester bath durable flame retardant is not environmentally friendly.
[0051] In the description of this specification, the description with reference to the terms "an experimental example", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the experimental example or example are included in at least one experimental example or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same experimental example or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more experimental examples or examples in a suitable manner.
[0052] Finally, it should be noted that the above experimental examples are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred experimental examples, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. An environmentally friendly durable flame retardant for polyester baths, It is characterized in that Its general structural formula is: The invention comprises the following raw materials in parts by weight: 75%-85% of N-dimethoxyphosphorylpropionylphthalimide, 5%-15% of anionic surfactant and 5%-20% of nonionic surfactant.
2. The environmentally friendly polyester bath durable flame retardant according to claim 1, It is characterized in that The anionic surfactants include one or more of dodecylbenzene sulfonic acid, sulfonated agricultural milk 600#, and sulfonated agricultural milk 600#F; the nonionic surfactants include one or more of agricultural milk 600#, fatty alcohol polyoxyethylene ether AEO-9, and fatty alcohol polyoxyethylene ether AEO-10.
3. A method for preparing an environmentally friendly durable flame retardant in polyester bath according to any one of claims 1-2, It is characterized in that After mixing N-dimethoxyphosphorylpropionylphthalimide with anionic surfactants and nonionic surfactants, the mixture is heated to 50-60° C. and kept warm for 20-40 minutes to obtain the environmentally friendly polyester bath durable flame retardant.
4. The method for preparing an environmentally friendly durable flame retardant in polyester bath according to claim 3, It is characterized in that The preparation steps of N-dimethoxyphosphoryl propionyl phthalimide are as follows: S1: dimethyl phosphite and acrylamide are first mixed, the temperature is raised to 50-60°C, sodium methoxide is used as a catalyst, and sodium methoxide is slowly added to the mixed solution of dimethyl phosphite and acrylamide to react, and dimethoxyphosphoryl propionamide is obtained after the reaction; S2 cools the temperature to 40-50° C., adds phthalic anhydride to the dimethoxyphosphoryl propionamide obtained in step S1, performs a ring-opening reaction, and then performs a dehydration ring-closing reaction to obtain N-dimethoxyphosphoryl propionyl phthalimide.
5. The method for preparing an environmentally friendly durable flame retardant in polyester bath according to claim 4, It is characterized in that In step S1, the molar ratio of dimethyl phosphite to acrylamide and sodium methoxide is 1:(1.05-1.15):(0.1-0.3).
6. The method for preparing an environmentally friendly durable flame retardant in polyester bath according to claim 4, It is characterized in that In step S2, the molar ratio of phthalic anhydride to dimethoxyphosphorylpropionamide is 1:(1.05-1.15).
7. The method for preparing an environmentally friendly durable flame retardant in polyester bath according to claim 4, It is characterized in that In step S1, when sodium methoxide is added to the mixed solution of dimethyl phosphite and acrylamide, the temperature is controlled at 71-80°C, and after the addition, the mixture is kept at 80-86°C for 3-5 hours to obtain dimethoxyphosphoryl propionamide.
8. The method for preparing an environmentally friendly durable flame retardant in polyester bath according to claim 4, It is characterized in that In step S2, phthalic anhydride is added to the dimethoxyphosphoryl propionamide obtained in step S1, and then the temperature is raised to 60-80° C. and kept warm for 1-3 hours to carry out a phthalic anhydride ring-opening reaction; after the reaction, the temperature is raised to 140-160° C. and a dehydration ring-closing reaction is carried out for 4-6 hours under a vacuum degree of -0.1-0.08 MPa.