Basalt fiber electromagnetic shielding paper with double-conductive network structure and preparation method of basalt fiber electromagnetic shielding paper

By forming a dual conductive network structure in basalt fiber electromagnetic shielding paper, the corrosion and weight problems of traditional electromagnetic shielding materials in extreme environments are solved, and efficient electromagnetic shielding performance and chemical stability are achieved, which are suitable for a variety of application scenarios.

CN118910919AActive Publication Date: 2024-11-08SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202411015310.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Traditional electromagnetic shielding materials have problems such as corrosion aging, heavy weight and high rigidity in extreme environments. The use of metal palladium catalysts in electroless plating technology poses potential harm to the environment and human health, making it difficult to meet the special needs in aerospace, military and other fields.

Method used

Basalt fiber electromagnetic shielding paper with a dual conductive network structure is formed by acid etching, coupling agent modification, electroless copper plating and nickel treatment, combined with aramid nanofibers to form a dual conductive network structure of composite paper, avoiding the traditional method. environmental pollution and health risks, and improve material stability and electromagnetic shielding efficiency.

Benefits of technology

It achieves efficient electromagnetic shielding performance in extreme environments, has excellent chemical stability and corrosion resistance, significantly improves electromagnetic interference shielding performance and Joule thermal performance, and is suitable for smart films, personal thermal management and wearable electromagnetic protection fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004965517780000011
    Figure HDA0004965517780000011
  • Figure HDA0004965517780000012
    Figure HDA0004965517780000012
  • Figure HDA0004965517780000021
    Figure HDA0004965517780000021
Patent Text Reader

Abstract

The invention provides basalt electromagnetic shielding paper with a double-conductive network structure and a preparation method of the basalt electromagnetic shielding paper. The preparation method comprises the following steps: carrying out modification and chemical copper plating treatment on basalt fibers; preparing an aramid nanofiber dispersion liquid; mixing with copper-plated basalt fibers, and preparing composite paper through vacuum-assisted filtration; and carrying out chemical nickel plating treatment on the composite paper to prepare the basalt electromagnetic shielding paper with the double-conductive network structure. Due to the construction of the double-conductive network structure, the basalt electromagnetic shielding paper not only has high electromagnetic shielding effectiveness of 40-90dB, but also shows the ratio (SE / t) of the high shielding effectiveness to the thickness of 800-2000dB mm <-1 > under the thickness of 0.02-0.2 mm. In addition, the basalt electromagnetic shielding paper with the double-conductive network structure also has excellent Joule thermal performance, and shows stable and lasting electromagnetic shielding performance in extreme environments (such as acid and alkali solutions, ignition, high and low temperature environments, ultrasonic cleaning and long-time storage).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the intersecting field of electromagnetic shielding materials and papermaking technology, and in particular to a basalt fiber electromagnetic shielding paper with a double conductive network structure and a preparation method thereof. Background Art

[0002] Chemical plating technology has the advantages of uniform coating, wide applicability and relatively low cost. However, the traditional chemical plating process using metal palladium as a catalyst has some potential hazards to the environment and human health. Therefore, it is crucial to find and develop an environmentally friendly and sustainable chemical plating method. At the same time, traditional electromagnetic shielding materials have disadvantages such as corrosion and aging in extreme environments. Traditional electromagnetic shielding materials have problems such as heavy weight and high rigidity, which may be limited in extreme environment applications with strict requirements on weight and flexibility. Therefore, finding new electromagnetic shielding materials with resistance to extreme environments has become an important direction of current research to meet the special needs of aerospace, military, energy and other fields for electromagnetic shielding in extreme environments.

[0003] Lightweight, high-performance, and multi-purpose applications of electromagnetic shielding materials have become an important development trend. Paper-based materials have a unique three-dimensional network structure with adjustable composition, structure, and thickness. As effective and practical materials for EMI (electromagnetic interference) shielding applications, they have attracted great attention, especially in portable devices, flexible protective materials, and aerospace.

[0004] BF (basalt fiber) is an emerging high-performance inorganic fiber with environmentally friendly and pollution-free characteristics, and is known as the "green industrial material of the 21st century". The fiber has high modulus, high strength, electrical insulation properties, excellent chemical stability, good heat resistance (-265℃-800℃), low thermal conductivity, and low moisture absorption. At present, BF is mainly used in the fields of wastewater treatment, sound absorption and wear-resistant materials, and the material has received continuous attention. So far, there are no reports on its application in electromagnetic shielding materials in extreme environments, and due to the smooth surface and chemical inertness of BF, the interface bonding in paper applications faces many challenges. Summary of the invention

[0005] The object of the present invention is to provide a double conductive network structure BF electromagnetic shielding paper and a preparation method thereof, using ANF (aramid nanofiber) as a reinforcing phase to improve the interface bonding problem of BF in paper-based materials.

[0006] To achieve the above purpose, the technical solution of the present invention is as follows:

[0007] A method for preparing a double conductive network structure BF electromagnetic shielding paper comprises the following steps:

[0008] (1) Acid etching of fiber surface: Prepare piranha solution to acid-etch BF;

[0009] (2) Coupling agent modification: The BF after acid etching in (1) is modified with an amino silane coupling agent;

[0010] (3) Activation: The BF modified in (2) is placed in an activation solution for activation treatment and cleaning, and then placed in a reducing agent solution for reduction treatment and cleaning;

[0011] (4) Plating: placing the BF obtained in (3) in a chemical plating solution for chemical copper plating to obtain a copper-plated basalt fiber mixed solution;

[0012] (5) mixing the copper-plated BF mixed solution and the ANF dispersion obtained in (4) to prepare a composite paper by a vacuum-assisted filtration method;

[0013] (6) activating and cleaning the composite paper prepared in (5), and then placing it in a reducing agent solution for reduction and cleaning;

[0014] (7) placing the composite paper obtained in (6) in a chemical plating solution for chemical nickel plating;

[0015] (8) Drying the nickel-plated composite paper in (7) to obtain a double conductive network electromagnetic shielding paper.

[0016] Furthermore, the piranha solution in (1) is H 2 SO 4 (sulfuric acid) and H 2 O 2 (hydrogen peroxide), the volume ratio is 1:1 to 3:1, the acid etching time is 0.5 to 2 hours, and the acid etching temperature is 70 to 100°C;

[0017] Further, the (2) is specifically as follows: firstly hydrolyzing an amino silane coupling agent with a mixed solution of ethanol and deionized water in a mass ratio of 1:1 to 10:1 to obtain an amino silane coupling agent solution with a concentration of 1 to 5 wt%, wherein the amino silane coupling agent comprises at least one of KH550, KH792, and KH602; then adding BF after acid etching for modification, wherein the concentration of BF after acid etching is 0.5 to 6 g / L, the modification temperature is 40 to 80° C., and the modification time is 8 to 24 h;

[0018] Furthermore, the composition of the chemical copper plating solution in (4) is 10-60 g / L EDTA-2Na (ethylenediaminetetraacetic acid disodium salt), 10-50 g / L NaKC 4 H4O 6 (potassium sodium tartrate), 5~25g / LCuSO 4 ·5H2 O (copper sulfate pentahydrate), 0.01~0.2g / LK 4 Fe(CN) 6 (potassium ferrocyanide), 10~60ml / L CH 2 O (formaldehyde), 0.01~0.5g / LC 10 H 8 N 2 (2-methyl-6-nitroquinoline);

[0019] Furthermore, the plating temperature is 40-80° C., the pH value of the copper plating solution is 10-12, and the plating time is 20-80 min.

[0020] Furthermore, the copper-plated BF content in the obtained mixed solution is 50-90wt%;

[0021] Furthermore, it is characterized in that the preparation method of the ANF dispersion in (5) is specifically: aramid fiber, KOH (potassium hydroxide), C 2 H 6 OS (dimethyl sulfoxide) and deionized water are mixed and stirred to crack the aramid fiber to form ANF, and then deionized water is added to perform protonation reduction reaction. After repeated washing, an ANF dispersion is obtained;

[0022] Furthermore, the activation solution in (3) and (6) includes AgNO 3 (silver nitrate) and deionized water, i.e., silver nitrate solution;

[0023] Furthermore, the reducing agent in (3) and (6) includes NaBH 4 (sodium borohydride) and deionized water, i.e., sodium borohydride solution;

[0024] Furthermore, the above (3) and (6) are specifically: immersing the modified BF in a AgNO solution having a concentration of 5 to 20 g / L 3 (silver nitrate) solution for 5 to 60 minutes, followed by rinsing with deionized water;

[0025] Further, the mixture is immersed in NaBH with a concentration of 20 to 50 g / L. 4 React in the solution for 10 to 30 minutes, and rinse again with deionized water;

[0026] Furthermore, the nickel plating solution in (7) is composed of 10 to 40 g / LC 6 H 5 Na 3 O 7 ·2H 2 O (sodium molybdate), 10-40 g / L NiSO 4 6H2 O (nickel sulfate hexahydrate), 5-20 g / L NaH 2 PO 2 ·H 2 O (sodium hypophosphite), 1-5 g / L DMAB (dimethylamine borane), 0.01-0.1 g / L SDS (sodium dodecyl sulfate);

[0027] Furthermore, the plating temperature is 30-80° C., the pH value of the nickel plating solution is 9-12, and the plating time is 10-100 min.

[0028] A double conductive network structure BF electromagnetic shielding paper, the thickness of the double conductive network electromagnetic shielding paper is 0.02-0.2 mm;

[0029] Furthermore, the double conductive network electromagnetic shielding paper has a total electromagnetic shielding effectiveness of 10 to 90 dB at a frequency of 8.2 to 12.4 GHz.

[0030] A double conductive network structure BF electromagnetic shielding paper is used as an intelligent film, personal thermal management or wearable electromagnetic protection field.

[0031] The above technical solution has the following advantages or beneficial effects:

[0032] The present invention provides a double conductive network structure BF electromagnetic shielding paper and a preparation method thereof. BF has the characteristics of high modulus, high strength, excellent chemical stability, good heat resistance, etc., but the surface of BF is smooth and chemically inert, and it is difficult to form surface bonding with other materials. The present invention adopts ANF as a reinforcing phase to improve the interface bonding problem of BF in paper-based materials.

[0033] Furthermore, the present invention uses the prepared piranha solution to perform acid etching on BF to make it rich in silanol groups.

[0034] Furthermore, a coupling agent surface modification technology is used to modify the etched BF with a silane coupling agent so that the BF can directly adsorb silver ions. This not only avoids the environmental pollution caused by the use of stannous chloride for sensitization in the prior art, but also reduces the number of operation steps.

[0035] Furthermore, BF adsorbs AgNO 3 The silver ions are coordinated with the amino groups and then reduced to silver nanoparticles, which serve as the catalytic center for subsequent chemical plating, thus avoiding the potential harm to the environment and human health caused by using metal palladium as a catalyst in the traditional chemical plating process; after that, chemical copper plating is carried out to prepare copper-plated BF.

[0036] Furthermore, ANF was prepared through a KOH system, and a copper-plated BF / ANF composite paper with a reinforced concrete layered structure was prepared using a vacuum-assisted filtration method; then, chemical nickel plating was performed through silver ion activation to form a double conductive network structure inside and on the surface of the composite paper; the copper-plated BF was used as the skeleton of the electromagnetic shielding paper and was interspersed between the ANFs to form a "reinforced concrete" structure, which improved the environmental stability of the composite paper under extreme conditions; a double conductive network structure was constructed inside and on the surface of the composite paper by chemical copper plating of BF and chemical nickel plating on the surface of the composite paper. Due to the synergistic effect of the double conductive network structure, the electromagnetic shielding effectiveness of the composite paper was significantly improved, that is, the composite paper not only had a 100-500S cm -1 It has high conductivity and high electromagnetic interference shielding effectiveness (EMI SE) of 40-90dB, and exhibits 800-2000dB mm at a thickness of 0.02-0.2mm. -1 High shielding effectiveness to thickness ratio (SE / t).

[0037] Furthermore, the composite paper consumes electromagnetic waves through electrical loss, magnetic loss and multiple reflection loss. Due to the excellent chemical stability of the nickel layer, it is wrapped on the surface of the composite paper to prevent the corrosion of the internal copper-plated fibers, effectively improving the extreme environmental stability of the composite paper. At the same time, thanks to the establishment of a double conductive network structure, the composite paper not only exhibits excellent electromagnetic shielding performance, but also has excellent Joule heating performance, and exhibits stable and lasting electromagnetic shielding performance in extreme environments (such as acid and alkaline solutions, ignition, high and low temperature environments, ultrasonic cleaning, and long-term storage). BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The following are SEM (field emission scanning electron microscope) images of copper-plated BF; (a) is the surface SEM image of copper-plated BF; (b) is the cross-sectional SEM image of copper-plated BF; (c) is the enlarged cross-sectional SEM image of copper-plated BF;

[0039] Figure 2 Surface and cross-sectional SEM images of 80 wt% copper-plated BF / ANF composite paper and nickel-plated composite paper; (a) is a surface SEM image of 80 wt% copper-plated BF / ANF composite paper; (b) is a cross-sectional SEM image of 80 wt% copper-plated BF / ANF composite paper; (c) is a surface SEM image of nickel-plated composite paper; (d) is a cross-sectional SEM image of nickel-plated composite paper;

[0040] Figure 3 The electromagnetic shielding effectiveness curve of 80wt% copper-plated BF / ANF composite paper;

[0041] Figure 4The shielding effectiveness curve of the composite paper treated with different nickel plating times;

[0042] Figure 5 The graph showing the change in electromagnetic shielding effectiveness of the composite paper with nickel plating only and the composite paper with a double conductive network structure;

[0043] Figure 6 Schematic diagram of the change of electromagnetic shielding effectiveness of the electromagnetic shielding paper with double conductive network structure under extreme environment; (a) is the change of electromagnetic shielding effectiveness of the composite paper after being immersed in acid and alkali solution for a period of time; (b) is the change of electromagnetic shielding effectiveness of the composite paper after being immersed in liquid nitrogen solution for a period of time; (c) is the change of electromagnetic shielding effectiveness of the composite paper after high-temperature annealing treatment; (d) is the change of electromagnetic shielding effectiveness of the composite paper after being ignited by an alcohol lamp; (e) is the change of electromagnetic shielding effectiveness of the composite paper after ultrasonic treatment; (f) is the change of electromagnetic shielding effectiveness of the composite paper after being placed for a period of time;

[0044] Figure 7 This is a temperature-time relationship diagram of the double conductive network structure composite paper when a gradient voltage is applied;

[0045] Figure 8 This is the tensile stress-strain diagram of the double conductive network structure composite paper after nickel plating for 20 minutes. DETAILED DESCRIPTION

[0046] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0047] A double conductive network electromagnetic shielding paper and a preparation method thereof, comprising the following specific steps:

[0048] (1) Acid etching of fiber surface: Prepare piranha solution to acid etch BF. The piranha solution is H 2 SO 4 and H 2 O 2 The volume ratio of the mixed solution is 1:1 to 3:1, the acid etching time is 0.5 to 2 hours, and the acid etching temperature is 70 to 100°C;

[0049] (2) Coupling agent modification: firstly, hydrolyze the amino silane coupling agent with a mixed solution of ethanol and deionized water in a mass ratio of 1:1 to 10:1 to obtain an amino silane coupling agent solution with a concentration of 1 to 5 wt%, wherein the amino silane coupling agent includes at least one of KH550, KH792, and KH602; then, add the BF after acid etching for modification, wherein the concentration of the BF after acid etching is 0.5 to 6 g / L, the modification temperature is 40 to 80° C., and the modification time is 8 to 24 h;

[0050] (3) Activation: The modified BF from (2) is immersed in AgNO with a concentration of 5 to 20 g / L. 3 (silver nitrate) solution for activation treatment, react for 5 to 60 minutes, then rinse with deionized water; then immerse in a 20 to 50 g / L NaBH 4 The solution was subjected to reduction treatment for 10 to 30 minutes, and then rinsed again with deionized water;

[0051] (4) Plating: The BF obtained in (3) is placed in a chemical plating solution for chemical copper plating. The composition of the chemical copper plating solution is 10-60 g / L EDTA-2Na, 10-50 g / L NaKC 4 H4O 6 , 5~25g / LCuSO 4 ·5H 2 O, 0.01~0.2g / LK 4 Fe(CN) 6 10~60ml / L CH 2 O, 0.01~0.5g / LC 10 H 8 N 2 , the plating temperature is 40-80°C, the pH value of the copper plating solution is 10-12, and the plating time is 20-80min to obtain a copper plating BF mixed solution;

[0052] (5) mixing the copper-plated BF mixed solution and the ANF dispersion obtained in (4) to prepare a composite paper by a vacuum-assisted filtration method;

[0053] (6) Immerse the composite paper prepared in (5) in a 5-20 g / L AgNO 3 The solution was activated for 5 to 60 minutes, followed by rinsing with deionized water; then immersed in a NaBH solution with a concentration of 20 to 50 g / L 4 The solution was subjected to reduction treatment for 10 to 30 minutes, and then rinsed again with deionized water;

[0054] (7) placing the composite paper obtained in (6) in a chemical plating solution for chemical nickel plating, wherein the nickel plating solution has a composition of 10 to 40 g / LC6 H 5 Na 3 O 7 ·2H 2 O, 10~40g / L NiSO 4 6H 2 O, 5~20g / LNaH 2 PO 2 ·H 2 O, 1-5 g / L DMAB, 0.01-0.1 g / L SDS, plating temperature is 30-80 ° C, pH value of nickel plating solution is 9-12, and plating time is 10-100 min;

[0055] (8) Drying the nickel-plated composite paper in (7) at a drying temperature of 80 to 120° C. for a drying time of 8 to 80 min to obtain a double conductive network electromagnetic shielding paper.

[0056] Preferably, the copper-plated BF content in the mixed solution obtained in (4) is 50-90wt%;

[0057] Preferably, the method for preparing the ANF dispersion in (5) is as follows: aramid fiber, KOH, C 2 H 6 OS and deionized water are mixed and stirred to crack the aramid fiber to form ANF, and then deionized water is added to perform a protonation reduction reaction. After repeated washing, an ANF dispersion is obtained.

[0058] A double conductive network structure BF electromagnetic shielding paper, the thickness of the double conductive network electromagnetic shielding paper is 0.02-0.2 mm;

[0059] Preferably, the double conductive network electromagnetic shielding paper has a total electromagnetic shielding effectiveness of 10 to 90 dB at a frequency of 8.2 to 12.4 GHz.

[0060] A double conductive network structure BF electromagnetic shielding paper is used as an intelligent film, personal thermal management or wearable electromagnetic protection field.

[0061] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0062] Embodiment 1:

[0063] The method for preparing the electromagnetic shielding paper with a double conductive network structure in this embodiment specifically comprises the following steps:

[0064] (1) Prepare a piranha solution to acid-etch BF. The piranha solution is H 2 SO 4 and H 2 O2 , the volume ratio is 7:3, the acid etching time is 1h, and the acid etching temperature is 90℃;

[0065] (2) Mix C in a certain proportion 2 H 5 OH and deionized water (C 2 H 5 OH: deionized water (mass ratio) = 9:1), and the mixed solution is used to hydrolyze KH-550 to obtain a KH-550 solution with a concentration of 1%; then, BF after acid etching is added thereto for modification, the concentration of BF after acid etching is 6 g / L, the modification temperature is 60° C., and the modification time is 12 h;

[0066] (3) Immerse the modified basalt in AgNO 3 The mixture was reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water and immersed in NaBH 4 The mixture was reacted in a solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0067] (4) Heat the chemical copper plating solution (500 mL) to 60°C and adjust the solution pH with 8M NaOH. When the pH reaches 10, add CH 2 O, stir thoroughly, then continue to add NaOH to raise the pH to 12; place the activated BF in (3) into the copper plating solution for reaction for 60 minutes; the copper plating solution composition is 40g / L EDTA-2Na, 30g / L NaKC 4 H4O 6 、16g / LCuSO 4 ·5H 2 O, 0.05g / LK 4 Fe(CN) 6 、40ml / LCH 2 O, 0.01g / LC 10 H 8 N 2 ;

[0068] (5) 1g aramid fiber, 1.5g KOH, 20ml deionized water, 500ml C 2 H 6 OS (mixed, magnetically stirred at room temperature for 4 hours, and finally a dark red ANF solution with a concentration of 0.2% was obtained. Then 41 ml of the ANF solution was measured and deionized water was injected into it under magnetic stirring. The mass ratio of the ANF solution to the deionized water was 1:2. After repeated washing, an ANF dispersion was obtained;

[0069] The copper-plated BF mixed solution obtained in (4) and the ANF dispersion solution in (5) are mixed, wherein the copper-plated BF content is 80 wt %, and a composite paper is prepared by a vacuum-assisted filtration method;

[0070] (6) Immerse the composite paper prepared in (5) in AgNO 3 The samples were reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water, and then immersed in a NaBH4 solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0071] (7) The composite paper prepared in (6) is then immersed in a plating solution (500 mL) to start a chemical nickel plating reaction; the specific nickel plating solution composition is 34 g / LC 6 H 5 Na 3 O 7 ·2H 2 O, 27g / LNiSO 4 6H 2 O, 15g / LNaH 2 PO 2 ·H 2 O, 3g / L DMAB, 0.01g / L SDS, through NH 3 ·H 2 O (ammonia water) adjusts the pH of the nickel plating solution to 10, maintains the plating solution temperature at 50°C, and reacts for 20 minutes;

[0072] (8) The nickel-plated composite paper obtained in (7) is dried at 105° C. for 10 min using a paper sample dryer to obtain a double conductive network electromagnetic shielding paper with a nickel plating time of 20 min.

[0073] like Figure 1 As shown, it is a SEM image of copper-plated BF. After chemical copper plating, the surface of BF is covered with dense copper particles, forming a dense and smooth coating. The copper layer is tightly bonded to the fiber, and the thickness of the coating is about 720nm.

[0074] like Figure 8 As shown, it is the tensile stress-strain diagram of the double conductive network structure composite paper plated with nickel for 20 minutes. The composite paper has good mechanical strength.

[0075] Embodiment 2:

[0076] The method for preparing the electromagnetic shielding paper with a double conductive network structure in this embodiment specifically comprises the following steps:

[0077] (1) Prepare a piranha solution to acid-etch BF. The piranha solution is H 2 SO 4 and H 2O 2 , volume ratio is 7:3, acid etching time is 1h, acid etching temperature is 90℃;

[0078] (2) Mix C in a certain proportion 2 H 5 OH and deionized water (C 2 H 5 OH: deionized water (mass ratio) = 9:1), and the mixed solution is used to hydrolyze KH-550 to obtain a KH-550 solution with a concentration of 1%; then, the acid-etched BF is added thereto for modification, the concentration of the acid-etched BF is 1 g / L, the modification temperature is 60° C., and the modification time is 12 h;

[0079] (3) Immerse the modified basalt in AgNO 3 The mixture was reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water and immersed in NaBH 4 The mixture was reacted in a solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0080] (4) Heat the chemical copper plating solution to 60°C and use 8M NaOH to adjust the solution pH. When the pH reaches 10, add CH 2 O, stir thoroughly, then continue to add NaOH to raise the pH to 12; place the activated BF in (3) into the copper plating solution for reaction for 60 minutes; the copper plating solution composition is 40g / L LEDTA-2Na, 30g / L NaKC 4 H4O 6 、16g / L CuSO 4 ·5H 2 O, 0.05g / LK 4 Fe(CN) 6 、40ml / L CH 2 O, 0.01g / LC 10 H 8 N 2 ;

[0081] (5) 1g aramid fiber, 1.5g KOH, 20ml deionized water, 500ml C 2 H 6 OS were mixed and magnetically stirred at room temperature for 4 hours to finally obtain a deep red ANF solution with a concentration of 0.2%. Then, 41 ml of the ANF solution was measured and deionized water was injected into it under magnetic stirring. The mass ratio of the aramid nanofiber solution to the deionized water was 1:2. After repeated washing, an ANF dispersion was obtained;

[0082] The copper-plated BF mixed solution obtained in (4) and the ANF dispersion solution in (5) are mixed, wherein the copper-plated BF content is 80 wt %, and a composite paper is prepared by a vacuum-assisted filtration method;

[0083] (6) Immerse the composite paper prepared in (5) in AgNO 3 The samples were reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water, and then immersed in a NaBH4 solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0084] (7) The composite paper prepared in (6) is then immersed in a plating solution (500 mL) to start a chemical nickel plating reaction; the specific nickel plating solution composition is 34 g / LC 6 H 5 Na 3 O 7 ·2H 2 O, 27g / L NiSO 4 6H 2 O, 15g / LNaH 2 PO 2 ·H 2 O, 3g / L DMAB, 0.01g / L SDS, by NH 3 ·H 2 O Adjust the pH of the nickel plating solution to 10, maintain the plating solution temperature at 50°C, and react for 40 minutes;

[0085] (8) The nickel-plated composite paper obtained in (7) is dried at 105° C. for 10 min using a paper sample dryer to obtain a double conductive network electromagnetic shielding paper with a nickel plating time of 40 min.

[0086] Embodiment 3:

[0087] The method for preparing the electromagnetic shielding paper with a double conductive network structure in this embodiment specifically comprises the following steps:

[0088] (1) Prepare a piranha solution to acid-etch BF. The piranha solution is H 2 SO 4 and H 2 O 2 , the volume ratio is 7:3, the acid etching time is 1h, and the acid etching temperature is 90℃;

[0089] (2) Mix C in a certain proportion 2 H 5 OH and deionized water (C 2 H 5OH: deionized water (mass ratio) = 9:1), and the mixed solution is used to hydrolyze KH-550 to obtain a KH-550 solution with a concentration of 1%; then, BF after acid etching is added thereto for modification, the concentration of BF after acid etching is 0.5 g / L, the modification temperature is 60° C., and the modification time is 12 h;

[0090] (3) Immerse the modified basalt in AgNO 3 The mixture was reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water and immersed in NaBH 4 The mixture was reacted in a solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0091] (4) Heat the chemical copper plating solution (500 mL) to 60°C and adjust the solution pH with 8M NaOH. When the pH reaches 10, add CH 2 O, stir thoroughly, then continue to add NaOH to raise the pH to 12; place the activated BF in (3) into the copper plating solution for reaction for 60 minutes; the copper plating solution composition is 40g / L EDTA-2Na, 30g / L NaKC 4 H4O 6 、16g / L CuSO 4 ·5H 2 O, 0.05g / LK 4 Fe(CN) 6 、40ml / L CH 2 O, 0.01g / LC 10 H 8 N 2 ;

[0092] (5) 1g aramid fiber, 1.5g KOH, 20ml deionized water, 500ml C 2 H 6 OS was mixed and magnetically stirred at room temperature for 4 hours to finally obtain a dark red ANF solution with a concentration of 0.2%. Then 41 ml of the ANF solution was measured and deionized water was injected into it under magnetic stirring. The mass ratio of the ANF solution to the deionized water was 1:2. After repeated washing, an ANF dispersion was obtained;

[0093] The copper-plated BF mixed solution obtained in (4) and the ANF dispersion solution in (5) are mixed, wherein the copper-plated BF content is 80 wt %, and a composite paper is prepared by a vacuum-assisted filtration method;

[0094] (6) Immerse the composite paper prepared in (5) in AgNO 3The samples were reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water, and then immersed in a NaBH4 solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0095] (7) The composite paper prepared in (6) is then immersed in a plating solution (500 mL) to start a chemical nickel plating reaction; the specific nickel plating solution composition is 34 g / LC 6 H 5 Na 3 O 7 ·2H 2 O, 27g / L NiSO 4 6H 2 O, 15g / L NaH 2 PO 2 ·H 2 O, 3g / L DMAB, 0.01g / L SDS, NH 3 ·H 2 O Adjust the pH of the nickel plating solution to 10, maintain the plating solution temperature at 50°C, and react for 60 minutes;

[0096] (8) The nickel-plated composite paper obtained in (7) is dried at 105° C. for 10 min using a paper sample dryer to obtain a double conductive network electromagnetic shielding paper with a nickel plating time of 60 min.

[0097] Embodiment 4:

[0098] The method for preparing the electromagnetic shielding paper with a double conductive network structure in this embodiment specifically comprises the following steps:

[0099] (1) Prepare a piranha solution to acid-etch BF. The piranha solution is H 2 SO 4 and H 2 O 2 , the volume ratio is 7:3, the acid etching time is 1h, and the acid etching temperature is 90℃;

[0100] (2) Mix C in a certain proportion 2 H 5 OH and deionized water (C 2 H 5 OH: deionized water (mass ratio) = 9:1), and the mixed solution is used to hydrolyze KH-550 to obtain a KH-550 solution with a concentration of 1%; then, BF after acid etching is added thereto for modification, the concentration of BF after acid etching is 3g / L, the modification temperature is 60°C, and the modification time is 12h;

[0101] (3) Immerse the modified basalt in AgNO 3The mixture was reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water and immersed in NaBH 4 The mixture was reacted in a solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0102] (4) Heat the chemical copper plating solution (500 mL) to 60°C and adjust the solution pH with 8M NaOH. When the pH reaches 10, add CH 2 O, stir thoroughly, then continue to add NaOH to raise the pH to 12; place the activated BF in (3) into the copper plating solution for reaction for 60 minutes; the copper plating solution composition is 40g / L EDTA-2Na, 30g / L NaKC 4 H4O 6 、16g / L CuSO 4 ·5H 2 O, 0.05g / LK 4 Fe(CN) 6 、40ml / L CH 2 O, 0.01g / LC 10 H 8 N 2 ;

[0103] (5) 1g aramid fiber, 1.5g KOH, 20ml deionized water, 500ml C 2 H 6 OS were mixed and magnetically stirred at room temperature for 4 hours to finally obtain a deep red ANF solution with a concentration of 0.2%. Then, 41 ml of the ANF solution was measured and deionized water was injected into it under magnetic stirring. The mass ratio of ANF to deionized water was 1:2. After repeated washing, an ANF dispersion was obtained;

[0104] The copper-plated BF mixed solution obtained in (4) and the ANF dispersion solution in (5) are mixed, wherein the copper-plated BF content is 80 wt %, and a composite paper is prepared by a vacuum-assisted filtration method;

[0105] (6) Immerse the composite paper prepared in (5) in AgNO 3 The samples were reacted in a solution (concentration of 10 g / L) for 30 min, then rinsed with deionized water, and then immersed in a NaBH4 solution (concentration of 40 g / L) for 15 min, and then rinsed with deionized water again;

[0106] (7) The composite paper prepared in (6) is then immersed in a plating solution (500 mL) to start a chemical nickel plating reaction; the specific nickel plating solution composition is 34 g / LC 6 H 5 Na 3 O 7 ·2H2 O, 27g / L NiSO 4 6H 2 O, 15g / LNaH 2 PO 2 ·H 2 O, 3g / L DMAB, 0.01g / L SDS, by NH 3 ·H 2 O Adjust the pH of the nickel plating solution to 10, maintain the plating solution temperature at 50°C, and react for 80 minutes;

[0107] (8) The nickel-plated composite paper obtained in (7) is dried at 105° C. for 10 min using a paper sample dryer to obtain a double conductive network electromagnetic shielding paper with a nickel plating time of 80 min.

[0108] like Figure 2 As shown, it is the SEM image of the surface and cross section of 80wt% copper-plated BF / ANF composite paper and nickel-plated composite paper. The copper-plated BF is interwoven inside as the skeleton of the composite paper to form a conductive network, while the ANF is filled between the copper-plated BF as a reinforcement phase to form a structure similar to "reinforced concrete";

[0109] Preferably, during the vacuum-assisted filtration process, a unique layered structure is formed, which extends the propagation path of the electromagnetic waves, thereby increasing the barrier effect on the electromagnetic waves;

[0110] Preferably, after the composite paper is nickel-plated, a dense nickel layer is formed on its surface, constructing a complete conductive network;

[0111] Preferably, this conductive network and the copper-plated BF inside the composite paper form a double conductive network structure, which effectively improves the loss of electromagnetic waves, thereby improving the electromagnetic shielding effectiveness of the composite paper. At the same time, the dense nickel layer has the characteristics of corrosion resistance and high temperature resistance, and is wrapped on the surface of the composite paper, effectively protecting the internal network structure and significantly improving the stability of the composite paper in extreme environments.

[0112] like Figure 3 As shown, it is the electromagnetic shielding effectiveness curve of 80wt% copper-plated BF / ANF composite paper. In the X-band, its average electromagnetic shielding effectiveness is 18.96dB.

[0113] like Figure 4 As shown in the figure, the shielding effectiveness curve of the composite paper treated with different nickel plating times is shown. As the nickel plating time increases, the electromagnetic shielding effectiveness of the composite paper gradually increases, from 40.7dB at 20min to 74dB at 80min.

[0114] like Figure 6 The figure is a schematic diagram of the change of electromagnetic shielding effectiveness of the double conductive network structure electromagnetic shielding paper under extreme environment;

[0115] Preferably, (a) shows the change in electromagnetic shielding effectiveness of electromagnetic shielding paper after being immersed in strong acid and alkali solutions for 24 hours. Since the external nickel layer provides effective protection, the electromagnetic shielding effectiveness of the sample does not change significantly, showing excellent corrosion resistance;

[0116] Preferably, (b-d) show the changes in electromagnetic shielding of the composite paper after being immersed in liquid nitrogen for 7 hours, placed in a 300°C tube furnace for 10 hours, and ignited under an alcohol lamp for 60 seconds;

[0117] Preferably, the results show that after these treatments, the electromagnetic shielding effectiveness of the samples remains above 80%;

[0118] Preferably, under the action of high-frequency mechanics, the electromagnetic shielding paper still exhibits a relatively satisfactory effect;

[0119] Preferably, (e) shows that after ultrasonic cleaning for 1 hour, the electromagnetic shielding effectiveness of the sample slightly decreases from 74dB to 68.04dB, with a retention rate of about 91%;

[0120] Preferably, (f) shows that after being stored at room temperature for 6 months, the electromagnetic shielding effectiveness of the composite paper still remains at 98%;

[0121] Preferably, these results illustrate that the double conductive network structure electromagnetic shielding paper has excellent electromagnetic shielding stability in extreme environments, mainly due to its double conductive network structure design and the superior performance of the nickel layer and nickel-plated BF, which makes the composite material exhibit significant environmental stability.

[0122] like Figure 7 As shown, this is a temperature-time relationship diagram of the double conductive network structure composite paper when a gradient voltage is applied. The composite paper has a rapid temperature response under different voltages, indicating that the composite paper has good temperature controllability.

[0123] Embodiment 5:

[0124] The method for preparing the electromagnetic shielding paper with a double conductive network structure in this embodiment specifically comprises the following steps:

[0125] (1) Prepare a piranha solution to acid-etch BF. The piranha solution is H 2 SO 4 and H 2 O 2 , the volume ratio is 1:1, the acid etching time is 0.5h, and the acid etching temperature is 70℃;

[0126] (2) Mix C in a certain proportion 2 H 5 OH and deionized water (C 2 H 5 OH: deionized water (mass ratio) = 1:1), and the mixed solution is used to hydrolyze KH-550 to obtain a KH-550 solution with a concentration of 5%; then, BF after acid etching is added thereto for modification, the concentration of BF after acid etching is 4g / L, the modification temperature is 40°C, and the modification time is 8h;

[0127] (3) Immerse the modified basalt in AgNO 3 The mixture was reacted in a solution (concentration of 5 g / L) for 5 min, then rinsed with deionized water and immersed in NaBH 4 The mixture was reacted in a solution (concentration of 20 g / L) for 10 min, and then rinsed with deionized water again;

[0128] (4) Heat the chemical copper plating solution (500 mL) to 40 °C, adjust the solution pH with 8 M NaOH, and add CH 2 O, stir thoroughly, then continue to add NaOH to raise the pH to 10; place the activated BF in (3) into the copper plating solution for reaction for 20 minutes; the copper plating solution composition is 10g / L LEDTA-2Na, 10g / L NaKC 4 H4O 6 , 5g / L CuSO 4 ·5H 2 O, 0.01g / LK 4 Fe(CN) 6 、10ml / L CH 2 O, 0.5g / LC 10 H 8 N 2 ;

[0129] (5) 1g aramid fiber, 1.5g KOH, 20ml deionized water, 500ml C 2 H 6 OS were mixed and magnetically stirred at room temperature for 4 hours to finally obtain a deep red ANF solution with a concentration of 0.2%. Then, 41 ml of the ANF solution was measured and deionized water was injected into it under magnetic stirring. The mass ratio of ANF to deionized water was 1:2. After repeated washing, an ANF dispersion was obtained;

[0130] The copper-plated BF mixed solution obtained in (4) and the ANF dispersion solution in (5) are mixed, wherein the copper-plated BF content is 50 wt %, and a composite paper is prepared by a vacuum-assisted filtration method;

[0131] (6) Immerse the composite paper prepared in (5) in AgNO3 The samples were then immersed in a 5 g / L NaBH4 solution for 10 min and then rinsed with deionized water.

[0132] (7) The composite paper prepared in (6) is then immersed in a plating solution (500 mL) to start a chemical nickel plating reaction; the specific nickel plating solution composition is 10 g / LC 6 H 5 Na 3 O 7 ·2H 2 O, 10g / L NiSO 4 6H 2 O, 5g / LNaH 2 PO 2 ·H 2 O, 1g / L DMAB, 0.1g / L SDS, by NH 3 ·H 2 O Adjust the pH of the nickel plating solution to 9, maintain the plating solution temperature at 30°C, and react for 10 minutes;

[0133] (8) The nickel-plated composite paper obtained in (7) is dried at 80° C. for 8 min using a paper sample dryer to obtain a double conductive network electromagnetic shielding paper with a nickel plating time of 10 min.

[0134] Embodiment 6:

[0135] The method for preparing the electromagnetic shielding paper with a double conductive network structure in this embodiment specifically comprises the following steps:

[0136] (1) Prepare a piranha solution to acid-etch BF. The piranha solution is H 2 SO 4 and H 2 O 2 , volume ratio is 3:1, acid etching time is 2h, acid etching temperature is 100℃;

[0137] (2) Mix C in a certain proportion 2 H 5 OH and deionized water (C 2 H 5 OH: deionized water (mass ratio) = 10:1), and the mixed solution is used to hydrolyze KH-550 to obtain a KH-550 solution with a concentration of 1%; then, BF after acid etching is added thereto for modification, the concentration of BF after acid etching is 1g / L, the modification temperature is 80°C, and the modification time is 24h;

[0138] (3) Immerse the modified basalt in AgNO 3The mixture was reacted in a solution (concentration of 20 g / L) for 60 min, then rinsed with deionized water and immersed in NaBH 4 The mixture was reacted in a solution (concentration of 50 g / L) for 30 min, and then rinsed with deionized water again;

[0139] (4) Heat the chemical copper plating solution (500 mL) to 80°C and adjust the solution pH with 8M NaOH. When the pH reaches 10, add CH 2 O, stir thoroughly, then continue to add NaOH to raise the pH to 12; place the activated BF in (3) into the copper plating solution for reaction for 80 minutes; the copper plating solution composition is 60g / L EDTA-2Na, 50g / L NaKC 4 H4O 6 、25g / L CuSO 4 ·5H 2 O, 0.2g / LK 4 Fe(CN) 6 、60ml / L CH 2 O, 0.01g / LC 10 H 8 N 2 ;

[0140] (5) 1g aramid fiber, 1.5g KOH, 20ml deionized water, 500ml C 2 H 6 OS (mixed, magnetically stirred at room temperature for 4 hours, and finally a dark red ANF solution with a concentration of 0.2% was obtained. Then 41 ml of the ANF solution was measured and deionized water was injected into it under magnetic stirring. The mass ratio of ANF to deionized water was 1:2. After repeated washing, an ANF dispersion was obtained;

[0141] The copper-plated BF mixed solution obtained in (4) and the ANF dispersion solution in (5) are mixed, wherein the copper-plated BF content is 90 wt %, and a composite paper is prepared by a vacuum-assisted filtration method;

[0142] (6) Immerse the composite paper prepared in (5) in AgNO 3 The samples were reacted in a 20 g / L solution for 60 min, then rinsed with deionized water, and then immersed in a 50 g / L NaBH4 solution for 30 min, and then rinsed with deionized water again;

[0143] (7) The composite paper prepared in (6) is then immersed in a plating solution (500 mL) to start a chemical nickel plating reaction; the specific nickel plating solution composition is 40 g / LC 6 H 5 Na 3 O 7 ·2H2 O, 40g / L NiSO 4 6H 2 O, 20g / LNaH 2 PO 2 ·H 2 O, 5g / L DMAB, 0.01g / L SDS, by NH 3 ·H 2 O Adjust the pH of the nickel plating solution to 12, maintain the plating solution temperature at 80°C, and react for 100 minutes;

[0144] (8) The nickel-plated composite paper obtained in (7) is dried at 120° C. for 80 min using a paper sample dryer to obtain a double conductive network electromagnetic shielding paper with a nickel plating time of 100 min.

[0145] Comparative Example 1:

[0146] In this comparative example, the only difference from Example 4 is that no copper-plated BF is added, and the composite paper is prepared only from ANF and then subjected to chemical nickel plating for 80 minutes.

[0147] like Figure 5 The figure shows the change in electromagnetic shielding effectiveness of composite paper plated with nickel only and composite paper with a double conductive network structure. Compared with the composite paper plated with nickel without copper-plated BF, the composite paper with a double conductive network structure shows more excellent electromagnetic shielding effectiveness under the same nickel plating time. Therefore, compared with the composite paper plated with nickel only, the synergistic effect of the nickel layer and the copper-plated BF gives the composite paper a more efficient conductive network and excellent electromagnetic shielding performance.

[0148] Test methods and conditions:

[0149] The scattering parameters (S11 and S21) in the frequency range of 8.2-12.4 GHz (X-band) were obtained by the waveguide method using a Rohde & Schwarz ZNB20 vector network analyzer, and the electromagnetic shielding performance of the composite paper was evaluated.

[0150] The power coefficients of reflection (R), transmission (T), and absorption (A), as well as the total EMI SE (SET), reflection SE (SER), and absorption SE (SEA) are calculated as follows:

[0151] R=|S 11 |2 (1)

[0152] T=|S 21 | 2 (2)

[0153] 1=A+R+T (3)

[0154] SE T =SEA +SE R +SE M (4)

[0155] SE R = -10log|1-R| (5)

[0156] SE A = -10log|T / (1-R)| (6)

[0157] Where SEM represents the multiple reflection SE between the two surfaces of the paper. If SET ≥ 15dB, SEM can be ignored. In addition, SE / t is used to represent the ratio of shielding effectiveness and thickness, where the unit of thickness is mm.

[0158] The morphological characteristics of the composite paper were analyzed using a field emission scanning electron microscope (SEM, TESCAN, 5kV). The tensile strength was evaluated using a tensile tester (AI-7000-NGD, Goodtechwell) at a speed of 5mm / min. The electrothermal conversion performance of the composite paper was studied at a certain voltage using a DC power supply (MS-6050, MAISHANG), and the temperature of the composite paper was measured using an infrared thermal imager (FLIRi7).

[0159] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper, characterized in that: The steps include: S1, acid etching of basalt fiber using piranha solution; S2, modifying the basalt fiber after acid etching in S1 with an amino silane coupling agent; S3, placing the basalt fiber modified by S2 in an activation solution for activation treatment and cleaning, and then placing it in a reducing agent solution for reduction treatment and cleaning; S4, placing the basalt fiber obtained in S3 in a chemical plating solution for chemical copper plating to obtain a copper-plated basalt fiber mixed solution; S5, mixing the copper-plated basalt fiber mixed solution obtained in S4 with the aramid nanofiber dispersion solution, and preparing a composite paper by a vacuum-assisted filtration method; S6, activating and washing the composite paper prepared in S5, and then placing the composite paper in a reducing agent solution for reduction and washing; S7, placing the composite paper obtained in S6 in a chemical plating solution for chemical nickel plating; S8, drying the nickel-plated composite paper obtained in S7 to obtain double conductive network electromagnetic shielding paper.

2. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The piranha solution in S1 is a mixture of sulfuric acid and hydrogen peroxide in a volume ratio of 1:1 to 3:1; the acid etching time is 0.5 to 2 hours, and the acid etching temperature is 70 to 100°C.

3. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The S2 is specifically as follows: firstly, an amino silane coupling agent is hydrolyzed with a mixed solution of ethanol and deionized water in a mass ratio of 1:1 to 10:1 to obtain an amino silane coupling agent solution with a concentration of 1 to 5 wt%, wherein the amino silane coupling agent includes at least one of KH550, KH792, and KH602; and then, acid-etched basalt fiber is added for modification, wherein the concentration of the acid-etched basalt fiber is 0.5 to 6 g / L, the modification temperature is 40 to 80°C, and the modification time is 8 to 24 hours.

4. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The composition of the chemical copper plating solution in S4 is 10-60 g / L LEDTA-2Na, 10-50 g / L NaKC4H4O6, 5-25 g / L CuSO4·5H2O, 0.01-0.2 g / L K4Fe(CN)6, 10-60 ml / L CHClO, 0.01-0.5 g / L CuSO4·5H2O, 10 H8N2, the plating temperature is 40-80°C, the pH value of the copper plating solution is 10-12, and the plating time is 20-80min; the content of copper-plated basalt fiber in the copper-plated basalt fiber mixed solution is 50-90wt%.

5. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The specific preparation process of the aramid nanofiber dispersion in S5 is: aramid fibers, potassium hydroxide, dimethyl sulfoxide and deionized water are mixed and stirred to crack the aramid fibers to form aramid nanofibers, and then deionized water is added to perform a protonation reduction reaction, and after repeated washing, the aramid nanofiber dispersion is obtained.

6. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The activation solution in S3 and S6 is a silver nitrate solution, and the reducing agent is a sodium borohydride solution; The S3 and S6 are specifically as follows: immersing the modified basalt fiber in a silver nitrate solution with a concentration of 5 to 20 g / L for reaction for 5 to 60 minutes, and then rinsing with deionized water; then immersing the modified basalt fiber in a sodium borohydride solution with a concentration of 20 to 50 g / L for reaction for 10 to 30 minutes, and rinsing with deionized water again.

7. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The nickel plating solution in S7 comprises 10-40 g / L C6H5Na3O7·2H2O, 10-40 g / L NiSO4·6H2O, 5-20 g / L NaH2PO2·H2O, 1-5 g / L DMAB, and 0.01-0.1 g / L SDS, the plating temperature is 30-80°C, the pH value of the nickel plating solution is 9-12, and the plating time is 10-100 min.

8. The method for preparing a double conductive network structure basalt fiber electromagnetic shielding paper according to claim 1, characterized in that: The drying treatment temperature in S8 is 80-120° C., and the drying treatment time is 8-80 min.

9. A basalt fiber electromagnetic shielding paper with a double conductive network structure, obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The thickness of the double conductive network electromagnetic shielding paper is 0.02-0.2 mm; the total electromagnetic shielding effectiveness of the double conductive network electromagnetic shielding paper for frequencies of 8.2-12.4 GHz is 10-90 dB.

10. Application of the double conductive network structure basalt fiber electromagnetic shielding paper according to claim 9 in the fields of smart film, personal thermal management or wearable electromagnetic protection.

Citation Information

Patent Citations

  • Carbon nanocomposite conductive paper and preparation method thereof

    CN108611918A

  • High-property fabric with high-temperature resistance and electric conductivity as well as preparation method thereof

    CN110230189A

  • Flexible composite electromagnetic shielding film constructed by utilizing conductive nanofibers and preparation method thereof

    CN113265908A

  • Basalt fiber continuous chemical plating device and application method

    CN114107963A

  • Conductive flame-retardant bending-resistant integrated composite yarn and preparation method thereof

    CN114635210A

Cited By

  • Friction material for noiseless low-abrasion electromagnetic brake and preparation method of friction material

    CN122059626A