Carbon steel / high-chromium cast iron composite bent pipe and method for detecting abrasion thickness of carbon steel / high-chromium cast iron composite bent pipe in non-destructive state
By leaving threaded through holes on the inner side of the carbon steel/high chromium cast iron composite bent pipe and using detection rods for wear thickness measurement, poor wear resistance and wear detection problems are solved, and the regular monitoring and replacement reminder of composite bent pipes is realized, which extends the Service life and improve production safety.
Patent Information
- Application Number
- CN202411152334.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
The existing wear-resistant composite bent pipes have problems such as poor wear resistance and difficult wear thickness in wear detection, which makes it difficult to evaluate the service life of the equipment, which may lead to material pipe penetration accidents and high production costs.
Carbon steel/high chromium cast iron composite bent pipe is used, and threaded through holes are reserved at the most bend on the inside. The wear thickness is measured in a non-destructive state through screws and scale detection rods with intermediate through holes, and wear is regularly monitored and recorded. In case, ensure the sealed state of the composite bent pipe.
It realizes regular monitoring of the wear status of composite bent pipes, extends service life, improves production safety and efficiency, and avoids equipment accidents and high replacement costs due to excessive wear.
Smart Images

Figure CN118912292A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wear thickness detection of wear-resistant elbow pipes in a non-destructive state, and specifically relates to a carbon steel / high-chromium cast iron composite elbow pipe and a method for detecting the wear thickness of the same in a non-destructive state. Background Art
[0002] With the development of industry, the requirements for material service life in actual production are increasing day by day. Some parts require materials to have both high hardness and excellent wear resistance, and at the same time, they are required to have good welding performance when connected with straight pipes. It is difficult for a single-component material to meet the above requirements at the same time.
[0003] In production conditions such as power and mining, during the transportation of materials such as coal powder and mineral materials, there are many bends in the steel pipes that need to be connected with elbows (also called "elbows"). Because coal powder, mineral materials and other materials have a certain hardness and scouring speed, the elbows are the parts that produce more serious wear. According to the material wear failure analysis when the elbows are used to transport materials, during the material transportation inside the pipeline, the material impact is mainly on the outer inner surface of the elbow, and after the material is refracted and reflected, it flows in the direction of the air supply or water flow (both called fluids). Therefore, the outer wall of the elbow is the most severely worn, while the inner wall of the elbow is almost not worn.
[0004] There are usually two types of existing wear-resistant composite elbows. One is to compound a layer of wear-resistant material inside the elbow through a vacuum negative pressure casting process (called "inner compound"). Due to the material conveying flow requirement inside the pipeline, the thickness of the inner composite wear-resistant layer is limited (10-15mm); the other is to compound a layer of wear-resistant material outside the elbow of the elbow through sand casting or vacuum negative pressure casting (called "outer compound"). The thickness of the outer composite wear-resistant layer can be increased to 40mm, thereby greatly improving the wear resistance of the elbow.
[0005] However, during the use of the above-mentioned wear-resistant composite material elbows, technicians and managers expect to be able to detect the degree of wear in a non-destructive state during the shutdown and maintenance of each main equipment, so as to regularly assess the service life of the elbows and replace them in time. Otherwise, there are several elbows in each operating system. After a certain period of use, the elbows will have material penetration due to severe wear, resulting in equipment and personnel safety accidents, as well as the production cost and production efficiency of the operating system that needs to be shut down for replacement. Summary of the invention
[0006] In order to solve the technical problems in the prior art that wear-resistant composite bent pipes have poor wear resistance and wear thickness is difficult to detect, the purpose of the present invention is to provide a carbon steel / high chromium cast iron composite bent pipe and a method for detecting wear thickness thereof in a non-destructive state. During the regular maintenance of industrial equipment, there is no need to disassemble or destroy the composite bent pipe body. By replacing the long screw containing a middle through hole reserved at the innermost bend of the inner side of the composite bent pipe, and inserting a preset detection rod marked with a scale into the middle through hole of the screw until the inner wall of the outer side of the composite bent pipe, the wear thickness is regularly measured to achieve regular monitoring of the wear state of the composite bent pipe. After measurement, the original screw without the middle hole is used to tighten the composite bent pipe to keep it sealed.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A carbon steel / high chromium cast iron bimetallic composite elbow comprises a carbon steel elbow and a wear-resistant layer composited on the outer surface of the carbon steel elbow, wherein the wear-resistant layer comprises a high chromium cast iron alloy layer composited on the outer surface of the carbon steel elbow and a carbon steel plate composited on the high chromium cast iron alloy layer.
[0009] The chemical formula of the high chromium cast iron alloy layer is 28CrMoCuB.
[0010] A method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite elbow in a non-destructive state comprises the following steps:
[0011] Step 1: A threaded through hole penetrating the pipe wall is provided at the most curved pipe wall on the side of the carbon steel pipe elbow away from the high chromium cast iron alloy layer;
[0012] Step 2: Process the middle of the screw into a through hole, and the length of the screw is at least greater than the wall thickness of the carbon steel elbow and smaller than the inner diameter of the carbon steel elbow;
[0013] Step 3: Place the screw with the middle through hole in step 2 into the threaded through hole in step 1; then insert the detection rod with a scale into the middle through hole of the screw until the front end of the detection rod touches the innermost bend of the carbon steel elbow close to the high chromium cast iron alloy layer, and record the straight-line distance displayed on the outer side of the pipe wall of the composite elbow away from the high chromium cast iron alloy layer;
[0014] Step 4: Before the composite bend is put into use, repeat step 3 to record the straight line distance L0 displayed on the outer side of the pipe wall of the composite bend away from the high chromium cast iron alloy layer, and record L0 as the standard length of the composite bend without wear;
[0015] Step 5: During equipment maintenance, the composite pipe bending material conveying is in a stopped state. Repeat step 3 to record the straight-line distance L displayed on the outer side of the pipe wall of the composite pipe bending away from the high chromium cast iron layer. n (n is a positive integer), calculate the wear thickness ΔL at each equipment maintenancen , that is, ΔL n =L n -L0.
[0016] In step 3, the length of the detection rod is at least greater than the sum of the thickness of the wear-resistant layer of the composite elbow and the outer diameter of the carbon steel elbow. The thickness of the wear-resistant layer of the composite elbow is the sum of the thickness of the high chromium cast iron alloy layer and the carbon steel plate.
[0017] The end of the detection rod away from the chromium cast iron alloy layer extends out of the inner pipe wall of the carbon steel elbow by at least 30 mm.
[0018] In step 3, the detection rod is adapted to the size of the through hole processed in the middle of the screw.
[0019] The method further includes:
[0020] Step 6: Based on the wear thickness ΔL during each equipment overhaul n , calculate the remaining thickness L of the wear-resistant layer of the composite elbow 剩 , the expression is as follows:
[0021] L 剩 =L 耐磨层 +D 碳钢弯管 -ΔL n
[0022] Among them, L 耐磨层 Indicates the wear-resistant layer thickness of the composite elbow, D 碳钢弯管 Indicates the wall thickness of the carbon steel elbow; according to the residual thickness L of the wear-resistant layer of the composite elbow 剩 Determine whether to replace the composite elbow;
[0023] Step 7: After each measurement, use a screw to tighten and seal the threaded through hole in step 1; the length of the screw is the same as the wall thickness of the carbon steel elbow.
[0024] If the remaining thickness of the wear-resistant layer of the composite elbow is L 剩 If the thickness is less than or equal to the working limit thickness of the wear-resistant layer of the composite elbow, replace the composite elbow in time.
[0025] The working limit thickness of the wear-resistant layer of the composite bent pipe is 5 mm.
[0026] The carbon steel bent pipe, screws and detection rod are all made of carbon steel Q235.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. Compared with the traditional rare earth wear-resistant steel elbow, the present invention improves the wear resistance of the carbon steel / high chromium cast iron bimetallic composite elbow by sequentially compounding a high chromium cast iron alloy layer and a carbon steel plate on the outside of the carbon steel elbow to form a carbon steel / high chromium cast iron wear-resistant composite elbow. The service life of the carbon steel / high chromium cast iron bimetallic composite elbow is 3 times that of the rare earth wear-resistant steel elbow, and the service life is greatly increased.
[0029] 2. The present invention reserves a threaded through hole at the innermost curved part of the composite bend pipe. On the one hand, it is used to tighten the composite bend pipe with the original screw without the middle hole under normal operating conditions to maintain the sealing state of the composite bend pipe; on the other hand, during the regular inspection and maintenance of industrial equipment, there is no need to disassemble or destroy the composite bend pipe body. Only by replacing the long screw with the middle through hole reserved at the innermost curved part of the composite bend pipe, a detection rod marked with a scale is inserted into the long screw with the middle through hole to measure the wear thickness of the outer side of the composite bend pipe, thereby realizing regular detection of the wear thickness of the composite bend pipe.
[0030] 3. The present invention is designed such that one end of the detection rod away from the chromium cast iron alloy layer extends out of the inner wall of the carbon steel elbow by at least 30 mm. When measuring the wear thickness of the outer inner wall of the composite elbow, the detection rod has a sufficient length for easy reading.
[0031] 4. The present invention inserts a detachable screw with a middle through hole into the threaded through hole reserved at the innermost bend of the composite bent pipe, and fixes the detection rod in the screw, thereby maintaining the straightness of the detection rod in the horizontal direction, and the measurement result is more accurate.
[0032] In summary, the wear thickness detection method of the present invention enables workers to perform regular inspections of industrial equipment without having to disassemble or destroy the composite bend pipe body. The workers only need to replace the long screw containing the middle through hole reserved at the innermost bend of the composite bend pipe, and use a marked detection rod to penetrate the middle through hole of the screw until the inner wall of the outer side of the composite bend pipe. The wear thickness is measured regularly, thereby achieving regular monitoring of the wear status of the composite bend pipe. After measurement, the composite bend pipe is tightened with the original screw without the middle hole to keep the composite bend pipe sealed. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 A schematic structural diagram of the carbon steel / high chromium cast iron bimetallic wear-resistant composite elbow provided by the present invention. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0035] A carbon steel / high chromium cast iron bimetallic composite elbow comprises a wear-resistant layer composited on the outer surface of the carbon steel elbow, wherein the wear-resistant layer comprises a high chromium cast iron alloy layer composited on the outer surface of the carbon steel elbow, and a carbon steel plate composited on the high chromium cast iron alloy layer.
[0036] The outer circumference of the carbon steel elbow is 240° composited with a high-chromium cast iron alloy layer, the chemical formula of the high-chromium cast iron alloy layer is 28CrMoCuB, the microhardness HV thereof is 1300-1400, and the macrohardness can reach HRC65; the microstructure of the high-chromium cast iron alloy layer includes eutectic carbide M7C3 and austenite and its transformation products, the morphology of the eutectic carbide M7C3 presents a chrysanthemum shape or a rod shape, and the eutectic carbide M7C3 as a wear-resistant hard phase has better toughness than ordinary white cast iron, and can be used in various abrasive wear, high temperature wear and corrosive wear conditions.
[0037] During the transportation process, the material in the carbon steel / high chromium cast iron bimetallic composite elbow will impact the inner pipe wall of the carbon steel elbow close to the high chromium cast iron alloy layer, causing serious wear of the inner pipe wall and affecting the normal use of the composite elbow. Therefore, it is necessary to regularly check the wear state of the composite elbow and replace it in time to prevent the composite elbow from being excessively worn and penetrating the pipe wall, thereby causing production accidents.
[0038] A method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe bend in a non-destructive state is used to detect the wear-resistant thickness of the carbon steel / high chromium cast iron bimetallic composite pipe bend, comprising the following steps:
[0039] Step 1: A threaded through hole penetrating the pipe wall is provided at the most curved pipe wall on the side of the carbon steel pipe elbow away from the high chromium cast iron alloy layer;
[0040] Step 2: Process the middle of the screw into a through hole, and the length of the screw is at least greater than the wall thickness of the carbon steel elbow and smaller than the inner diameter of the carbon steel elbow;
[0041] Step 3: Place the screw with the middle through hole in step 2 into the threaded through hole in step 1; then insert a detection rod with a scale into the middle through hole of the screw until the front end of the detection rod contacts the innermost bend of the carbon steel elbow close to the high chromium cast iron alloy layer, and record the straight-line distance displayed on the outer side of the pipe wall of the composite elbow away from the high chromium cast iron alloy layer; the length of the detection rod is at least greater than the sum of the thickness of the wear-resistant layer of the composite elbow and the outer diameter of the carbon steel elbow, and the thickness of the wear-resistant layer of the composite elbow is the sum of the thickness of the high chromium cast iron alloy layer and the carbon steel plate;
[0042] In order to have sufficient length to facilitate reading when measuring the wear thickness of the inner wall of the outer side of the composite elbow, the end of the detection rod away from the chromium cast iron alloy layer extends out of the inner wall of the carbon steel elbow by at least 30 mm;
[0043] Step 4: Before the composite bend is put into use, repeat step 3 to record the straight line distance L0 displayed on the outer side of the pipe wall of the composite bend away from the high chromium cast iron alloy layer, and record L0 as the standard length of the composite bend without wear;
[0044] The size of the through hole processed between the detection rod and the screw is adapted;
[0045] Step 5: During equipment maintenance, the composite pipe bending material conveying is in a stopped state. Repeat step 3 to record the straight-line distance L displayed on the outer side of the pipe wall of the composite pipe bending away from the high chromium cast iron layer. n (n is a positive integer), calculate the wear thickness ΔL at each equipment maintenance n , that is, ΔL n =L n -L0;
[0046] Step 6: Based on the wear thickness ΔL during each equipment overhaul n , calculate the remaining thickness L of the wear-resistant layer of the composite elbow 剩 , the expression is as follows:
[0047] L 剩 =L 耐磨层 +D 碳钢弯管 -ΔL n
[0048] Among them, L 耐磨层 Indicates the wear-resistant layer thickness of the composite elbow, D 碳钢弯管 Indicates the wall thickness of the carbon steel elbow; according to the residual thickness L of the wear-resistant layer of the composite elbow 剩 Determine whether to replace the composite elbow;
[0049] If the remaining thickness of the wear-resistant layer of the composite elbow is L 剩 If the working limit thickness of the wear-resistant layer of the composite elbow pipe is less than or equal to the working limit thickness, the composite elbow pipe should be replaced in time to ensure production safety; the working limit thickness of the wear-resistant layer of the composite elbow pipe is preferably 5mm;
[0050] Step 7: After each measurement, the threaded through hole in step 1 is tightened and sealed with a screw to maintain the sealing state of the composite elbow; the length of the screw is the same as the wall thickness of the carbon steel elbow.
[0051] The carbon steel bent pipe, screws and detection rod are all made of carbon steel Q235.
[0052] Example 1
[0053] The method for detecting the wear-resistant thickness of the carbon steel / high chromium cast iron bimetallic composite elbow for coal transportation in Lueyang thermal power plant under non-destructive conditions includes the following steps:
[0054] Step 1: A threaded through hole penetrating the pipe wall is provided at the most curved pipe wall of the carbon steel pipe of the composite pipe bend on the side away from the high chromium cast iron layer; the size specification of the threaded through hole is M10×1;
[0055] Step 2: Process the middle of the screw into a through hole with a diameter of 6mm; the length of the screw is 40mm, which is the same as the size specification of the threaded through hole, that is, M10×1;
[0056] Step 3: Place the screw with the middle through hole in step 2 into the threaded through hole in step 1; then insert the detection steel rod with scale into the middle through hole of the screw until the front end of the detection rod touches the inner wall of the carbon steel pipe at the side close to the high chromium cast iron layer; the diameter of the detection steel rod is 6 -0.5 mm;
[0057] The outer diameter of the carbon steel pipe of the composite elbow used in this working condition is 450mm, the thickness of the carbon steel pipe wall is 10mm, the thickness of the high chromium cast iron layer is 35mm, and the thickness of the carbon steel plate is 6mm. Therefore, the thickness of the wear-resistant layer of the composite elbow is 41mm, and the length of the detection steel rod is at least 491mm. In order to further facilitate the reading of the detection personnel, the length of the detection steel rod is set to 520mm;
[0058] Step 4: Before the composite bend is put into use, repeat step 3 to record the straight-line distance L0 = 450-10 = 440 mm displayed on the outer side of the pipe wall of the composite bend away from the high-chromium cast iron layer, and record L0 as the standard length of the composite bend without wear;
[0059] Step 5: During the first overhaul of the equipment, the material conveying of the composite pipe bend is in a stopped state. Repeat step 3 to record the straight-line distance L1=442mm displayed on the outer side of the pipe wall of the composite pipe bend away from the high-chromium cast iron layer, and the corresponding wear thickness ΔL1=442-440=2mm;
[0060] During the 18th equipment maintenance, record the straight-line distance L shown on the outer side of the pipe wall of the composite bend away from the high chromium cast iron layer. 18 =487mm, corresponding to the wear thickness ΔL 18 =487-440=47mm;
[0061] Step 6: Based on the wear thickness ΔL during each equipment overhaul n , calculate the remaining thickness L of the wear-resistant layer of the composite elbow 剩 , the expression is as follows:
[0062] L 剩 =L 耐磨层 +D 碳钢弯管 -ΔL n
[0063] Among them, L 耐磨层 Indicates the wear-resistant layer thickness of the composite elbow, D 碳钢弯管 Indicates the wall thickness of the carbon steel elbow; according to the residual thickness L of the wear-resistant layer of the composite elbow 剩 Determine whether to replace the composite elbow;
[0064] If the remaining thickness of the wear-resistant layer of the composite elbow is L 剩 If the working limit thickness of the wear-resistant layer of the composite elbow pipe is less than or equal to the working limit thickness, the composite elbow pipe should be replaced in time to ensure production safety; the working limit thickness of the wear-resistant layer of the composite elbow pipe is preferably 5mm;
[0065] When the equipment is overhauled for the first time, the remaining thickness L of the wear-resistant layer of the composite elbow 剩 It is 41+10-2=49mm, which is greater than the working limit thickness of the wear-resistant layer of the composite elbow 5mm, and the composite elbow can continue to be used;
[0066] When the equipment was overhauled for the eighteenth time, the remaining thickness of the wear-resistant layer of the composite elbow was L 剩 It is 41+10-47=4mm, which is less than the working limit thickness of the wear-resistant layer of the composite elbow 5mm. In order to ensure production safety, the composite elbow is replaced;
[0067] Step 7: After each measurement, use a screw (M10×1) of the same specification as the threaded through hole in step 1 to tighten and seal the threaded through hole in step 1 to maintain the sealing state of the composite elbow; the length of the screw is the same as the wall thickness of the carbon steel elbow.
[0068] The specific measurement data are shown in Table 1:
[0069] Table 1 Wear-resistant thickness of rare earth wear-resistant steel elbow and carbon steel / high chromium cast iron bimetallic composite elbow
[0070]
[0071] Example 2
[0072] The method for detecting the wear-resistant thickness of the carbon steel / high chromium cast iron bimetallic composite elbow pipe for coal transportation in Hancheng thermal power plant under non-destructive conditions includes the following steps:
[0073] Step 1: A threaded through hole penetrating the pipe wall is provided at the most curved pipe wall of the carbon steel pipe of the composite pipe bend on the side away from the high chromium cast iron layer; the size specification of the threaded through hole is M10×1;
[0074] Step 2: Process the middle of the screw into a through hole with a diameter of 6mm; the length of the screw is 40mm, which is the same as the size specification of the threaded through hole, that is, M10×1;
[0075] Step 3: Place the screw with the middle through hole in step 2 into the threaded through hole in step 1; then insert the detection steel rod with scale into the middle through hole of the screw until the front end of the detection rod touches the inner wall of the carbon steel pipe at the side close to the high chromium cast iron layer; the diameter of the detection steel rod is 6 -0.5 mm;
[0076] The outer diameter of the carbon steel pipe of the composite elbow used in this working condition is 420mm, the thickness of the carbon steel pipe wall is 10mm, the thickness of the high chromium cast iron layer is 35mm, and the thickness of the carbon steel plate is 6mm. Therefore, the thickness of the wear-resistant layer of the composite elbow is 41mm, and the length of the detection steel rod is at least 461mm. In order to further facilitate the reading of the detection personnel, the length of the detection steel rod is set to 490mm;
[0077] Step 4: Before the composite bend is put into use, repeat step 3 to record the straight line distance L0 = 420-10 = 410 mm displayed on the outer side of the pipe wall of the composite bend away from the high chromium cast iron layer, and record L0 as the standard length of the composite bend without wear;
[0078] Step 5: During the first overhaul of the equipment, the material conveying of the composite pipe bend is in a stopped state. Repeat step 3 to record the straight-line distance L1=418mm displayed on the outer side of the pipe wall of the composite pipe bend away from the high-chromium cast iron layer, and the corresponding wear thickness ΔL1=418-410=8mm;
[0079] During the 18th equipment maintenance, record the straight-line distance L shown on the outer side of the pipe wall of the composite bend away from the high chromium cast iron layer. 18 =456.5mm, corresponding to the wear thickness
[0080] ΔL 18 =456.5-410=46.5mm;
[0081] Step 6: Based on the wear thickness ΔL during each equipment overhaul n , calculate the remaining thickness L of the wear-resistant layer of the composite elbow 剩 , the expression is as follows:
[0082] L 剩 =L 耐磨层 +D 碳钢弯管 -ΔL n
[0083] Among them, L 耐磨层 Indicates the wear-resistant layer thickness of the composite elbow, D 碳钢弯管 Indicates the wall thickness of the carbon steel elbow; according to the residual thickness L of the wear-resistant layer of the composite elbow 剩 Determine whether to replace the composite elbow;
[0084] If the remaining thickness of the wear-resistant layer of the composite pipe bend is not greater than the working limit thickness of the wear-resistant layer of the composite pipe bend, the composite pipe bend is replaced in time to ensure production safety; the working limit thickness of the wear-resistant layer of the composite pipe bend is preferably 5 mm;
[0085] When the equipment is overhauled for the first time, the remaining thickness L of the wear-resistant layer of the composite elbow 剩It is 41+10-8=43mm, which is greater than the working limit thickness of the wear-resistant layer of the composite elbow 5mm, and the composite elbow can continue to be used;
[0086] When the equipment was overhauled for the eighteenth time, the remaining thickness of the wear-resistant layer of the composite elbow was L 剩 It is 41+10-46.5=4.5mm, which is less than the working limit thickness of the wear-resistant layer of the composite elbow 5mm. In order to ensure production safety, the composite elbow is replaced;
[0087] Step 7: After each measurement, use a screw (M10×1) of the same specification as the threaded through hole in step 1 to tighten and seal the threaded through hole in step 1 to maintain the sealing state of the composite elbow; the length of the screw is the same as the wall thickness of the carbon steel elbow.
[0088] The specific measurement data are shown in Table 2:
[0089] Table 2 Wear-resistant thickness of rare earth wear-resistant steel elbow and carbon steel / high chromium cast iron bimetallic composite elbow
[0090]
[0091]
[0092] It can be seen from Tables 1 and 2 that, compared with the rare earth wear-resistant steel elbow, the service life of the carbon steel / high chromium cast iron bimetallic composite elbow is 3 times that of the rare earth wear-resistant steel elbow, indicating that the wear resistance of the carbon steel / high chromium cast iron bimetallic composite elbow is better; at the same time, the wear-resistant thickness detection method of the present invention realizes regular monitoring of the wear state of the composite elbow under non-destructive conditions, and gives a warning when the wear thickness reaches or approaches the working limit thickness of the composite elbow, reminding the staff to replace the severely worn composite elbow in time, effectively preventing the occurrence of production safety accidents.
[0093] The wear-resistant layer thickness detected by the wear-resistant thickness detection method of the present invention can be accurate to 0.1mm; by repeatedly detecting the wear thickness of the outer wall of the composite elbow, it can be gradually detected whether the remaining thickness of the outer wall of the elbow is equal to or less than 5mm, and a warning can be given and replaced in time.
Claims
1. A carbon steel / high chromium cast iron bimetallic composite elbow, Features: The invention comprises a carbon steel elbow and a wear-resistant layer compounded on the outer surface of the carbon steel elbow. The wear-resistant layer comprises a high-chromium cast iron alloy layer compounded on the outer surface of the carbon steel elbow and a carbon steel plate compounded on the high-chromium cast iron alloy layer.
2. A carbon steel / high chromium cast iron bimetallic composite elbow according to claim 1, Features: The chemical formula of the high chromium cast iron alloy layer is 28CrMoCuB.
3. A method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe bend in a non-destructive state according to claim 1 or 2, It is characterized in that The following steps are involved: Step 1: A threaded through hole penetrating the pipe wall is provided at the most curved pipe wall on the side of the carbon steel pipe elbow away from the high chromium cast iron alloy layer; Step 2: Process the middle of the screw into a through hole, and the length of the screw is at least greater than the wall thickness of the carbon steel elbow and smaller than the inner diameter of the carbon steel elbow; Step 3: Place the screw with the middle through hole in step 2 into the threaded through hole in step 1; then insert the detection rod with a scale into the middle through hole of the screw until the front end of the detection rod touches the innermost bend of the carbon steel elbow close to the high chromium cast iron alloy layer, and record the straight-line distance displayed on the outer side of the pipe wall of the composite elbow away from the high chromium cast iron alloy layer; Step 4: Before the composite bend is put into use, repeat step 3 and record the straight-line distance L displayed on the outer side of the composite bend away from the high-chromium cast iron alloy layer. 0 , L 0 It is recorded as the standard length of the composite elbow without wear; Step 5: During equipment maintenance, the composite pipe bending material conveying is in a stopped state. Repeat step 3 to record the straight-line distance L displayed on the outer side of the pipe wall of the composite pipe bending away from the high chromium cast iron layer. n (n is a positive integer), calculate the wear thickness ΔL at each equipment maintenance n , that is, ΔL n =L n -L 0 .
4. According to claim 3, a method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite elbow in a non-destructive state, Features: In step 3, the length of the detection rod is at least greater than the sum of the thickness of the wear-resistant layer of the composite elbow and the outer diameter of the carbon steel elbow. The thickness of the wear-resistant layer of the composite elbow is the sum of the thickness of the high chromium cast iron alloy layer and the carbon steel plate.
5. The method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe elbow in a non-destructive state according to claim 4, Features: The end of the detection rod away from the chromium cast iron alloy layer extends out of the inner pipe wall of the carbon steel elbow by at least 30 mm.
6. The method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe elbow in a non-destructive state according to claim 3, Features: In step 3, the detection rod is adapted to the size of the through hole processed in the middle of the screw.
7. The method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe elbow in a non-destructive state according to claim 3, It is characterized in that The method further includes: Step 6: Based on the wear thickness ΔL during each equipment overhaul n , calculate the remaining thickness L of the wear-resistant layer of the composite elbow 剩 , the expression is as follows: L 剩 =L 耐磨层 +D 碳钢弯管 -ΔL n Among them, L 耐磨层 Indicates the wear-resistant layer thickness of the composite elbow, D 碳钢弯管 Indicates the wall thickness of the carbon steel elbow; according to the residual thickness L of the wear-resistant layer of the composite elbow 剩 Determine whether to replace the composite elbow; Step 7: After each measurement, use a screw to tighten and seal the threaded through hole in step 1; the length of the screw is the same as the wall thickness of the carbon steel elbow.
8. The method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe elbow in a non-destructive state according to claim 7, Features: If the remaining thickness of the wear-resistant layer of the composite elbow is L 剩 If the thickness is less than or equal to the working limit thickness of the wear-resistant layer of the composite elbow, replace the composite elbow in time.
9. The method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe elbow in a non-destructive state according to claim 7, Features: The working limit thickness of the wear-resistant layer of the composite bent pipe is 5 mm.
10. The method for detecting the wear-resistant thickness of a carbon steel / high chromium cast iron bimetallic composite pipe elbow in a non-destructive state according to claim 3, Features: The carbon steel bent pipe, screws and detection rod are all made of carbon steel Q235.