Method for testing internal residual stress distribution of environmental barrier coating

Through the in-situ quantization method of micro Raman spectroscopy, the problem of inaccurate residual stress measurement within the environmental barrier coating is solved, high-precision and lossless stress distribution measurement is achieved, and the reliability of the coating is improved in high-temperature corrosion environment.

CN118913495APending Publication Date: 2024-11-08BEIJING INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410705962.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art cannot accurately measure the residual stress distribution inside the environmental barrier coating, resulting in inaccurate measurement and large errors, affecting the reliability of the coating in a high-temperature corrosion environment.

Method used

The Raman shift-stress factor of the coating was measured by the in-situ quantization method of micro Raman spectroscopy, and the residual stress state of the test area was determined based on the linear relationship between the coating Raman signal and the Raman shift. Microscopy was used to determine the residual stress state of the test area. A confocal Raman spectrometer performs high resolution measurements with a laser beam spot diameter of less than 1 μm.

Benefits of technology

It realizes high-precision, non-destructive and in-situ measurement of the residual stress distribution inside the environmental barrier coating, provides accurate stress distribution data in the microscopic area of ​​the coating, and improves the reliability and long-term service capability of the coating in high-temperature corrosion environments. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913495A_ABST
    Figure CN118913495A_ABST
Patent Text Reader

Abstract

The invention discloses a method for testing internal residual stress distribution of an environmental barrier coating, which comprises the following steps of: S1, measuring a Raman frequency shift-stress factor of a substrate in the environmental barrier coating through a stretching method, and calibrating the Raman frequency shift-stress factor of each coating layer by layer in situ; and S2, according to the Raman frequency shift-stress factor, determining the residual stress state of the test area based on the linear relationship between the coating Raman signal and the Raman frequency shift. By adopting the technical scheme of the invention, the problems of inaccurate measurement of the residual stress of the coating, random test result and large error are solved, the residual stress of the microscopic area of the section of the coating can be measured in situ in a nondestructive manner, and the method has high precision and resolution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of environmental barrier coatings, and in particular relates to a method for testing the internal residual stress distribution of environmental barrier coatings based on in-situ quantification of micro-Raman spectroscopy. Background Art

[0002] Environmental barrier coatings are used as advanced high-temperature corrosion protection technologies to protect hot-end components in the field of aero-engines and gas turbines. However, during the preparation and service stage of environmental barrier coatings, the thermal expansion mismatch between the coating and the components and the corrosion of the coating by external substances will cause residual stress inside the coating. Stress concentration will lead to cracks and even coating peeling, which is one of the main reasons for coating failure. Therefore, accurately measuring the residual stress distribution in environmental barrier coatings to prevent cracks and failure of the coating is of great significance for environmental barrier coatings to protect hot-end components from high-temperature corrosion environments and improve their reliability in long-term service at high temperatures.

[0003] At present, there are many methods for measuring the residual stress of environmental barrier coatings, such as X-ray diffraction, micro-focused high-energy X-ray diffraction, and combined X-ray-Raman method. The X-ray diffraction method and micro-focused high-energy X-ray diffraction have the same principle. X-rays are used to diffract on the coating surface to measure the strain caused by the change in lattice spacing on the coating surface, thereby calculating the average stress level near the test position. The measurement accuracy and penetration ability of X-rays are limited, and only the stress value of the material surface can be roughly measured. The micro-focused high-energy X-ray diffraction method has strong penetration ability and high measurement accuracy, but its measurement cost is high and cannot be widely used in actual measurement. The X-ray-Raman method measures the stress value of the coating surface through X-ray diffraction, calculates the Raman frequency shift-stress factor by comparing it with the Raman peak frequency shift, and then calculates the residual stress by the Raman frequency shift-stress factor and the Raman frequency shift. This method has the same defects as X-ray measurement. Affected by the X-ray measurement accuracy, the Raman frequency shift-stress factor measured by this method has a large error, which affects the judgment of the actual stress of the coating.

[0004] Therefore, how to accurately measure the residual stress distribution of environmental barrier coatings is of great significance to avoid failure of the coatings in high-temperature corrosion environments and thus protect the hot end components. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for testing the internal residual stress distribution of an environmental barrier coating, which solves the problems of inaccurate measurement of the residual stress of the coating and random test results with large errors. The method can non-destructively measure the residual stress in the microscopic area of ​​the coating cross section in situ with high accuracy and resolution.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A method for testing residual stress distribution inside an environmental barrier coating, comprising:

[0008] Step S1, measuring the Raman frequency shift-stress factor of the substrate in the environmental barrier coating by a tensile method, and calibrating the Raman frequency shift-stress factor of each coating layer by layer in situ;

[0009] Step S2: determining the residual stress state of the test area according to the Raman frequency shift-stress factor and based on the linear relationship between the coating Raman signal and the Raman frequency shift.

[0010] Preferably, the environmental barrier coating system comprises a substrate, a bonding layer and an environmental barrier coating; the substrate material is silicon carbide and its composite materials, silicon nitride and its composite materials; the bonding layer is silicon and its modified materials; and the environmental barrier coating is rare earth silicate or corrosion-related coating materials.

[0011] The present invention also provides a method for testing the residual stress distribution inside an environmental barrier coating, comprising:

[0012] Obtain the initial Raman absorption peak wave number ω0 of the environmental barrier coating material in a stress-free state;

[0013] Measurement of Raman frequency shift-stress factor R of substrate by stretching method E :

[0014] After cold cutting and polishing, the coating to be tested is cut to obtain a smooth cross section, and the coating cross section is imaged by a microscope system to select the area to be tested;

[0015] Use a micro-Raman spectrometer to collect Raman signals from the stress distribution area to be tested;

[0016] According to the Raman frequency shift of the substrate-stress factor R E Calculate the Raman frequency shift-stress factor R1 of the adjacent bonding layer, calculate the Raman frequency shift-stress factor R2 of the adjacent coating based on the Raman frequency shift-stress factor of the bonding layer, and calculate the Raman frequency shift-stress factor R of the i-th coating layer. i ;

[0017] According to the Raman signal collected in the test area and the initial Raman absorption peak wave number ω0, the Raman frequency shift Δω of each acquisition point in each layer is calculated. i ;

[0018] According to the Raman frequency shift of each layer of material-stress factor R i and the Raman frequency shift Δω i , calculate the stress state of each test point;

[0019] The stress state of each test point is imaged to obtain the quantitative results of the stress distribution at the corresponding position of the test area.

[0020] Preferably, the environmental barrier coating system comprises a substrate, a bonding layer and an environmental barrier coating; the substrate material is silicon carbide and its composite materials, silicon nitride and its composite materials; the bonding layer is silicon and its modified materials; and the environmental barrier coating is rare earth silicate or corrosion-related coating materials.

[0021] As a preference, the Raman frequency shift-stress factor R of the substrate is measured. E as follows:

[0022]

[0023] Where F is the tensile force on the substrate, S is the stretched cross-sectional area, Δω E =ω E -ω E0 It represents the frequency shift between the actual Raman absorption peak wavenumber of the matrix and the standard absorption peak wavenumber.

[0024] As a preference, the Raman frequency shift-stress factor R of each layer of material is i , the stress state of each test point is calculated,

[0025] σ i =R i (ω i -ω i0 )

[0026] Preferably, the stress state of each point after imaging is determined by the positive and negative signs of the numerical results after quantification, where a positive sign indicates tensile stress and a negative sign indicates compressive stress.

[0027] Preferably, the minimum laser beam spot diameter for collecting Raman signals is less than 1 μm.

[0028] In the method of the present invention, since the coating itself is relatively thin, the Raman frequency shift-stress factor R is measured by the stretching method. i It is not easy to achieve. The Raman frequency shift-stress factor R calculated by the method of the present invention i It is obtained in situ based on the data collected from the coating to be tested, and is not affected by the coating preparation method and the coating microstructure, so the method of obtaining it is more flexible and accurate. The laser beam spot diameter of the microscopic confocal Raman spectrometer used in the method of the present invention is less than 1μm, so the test result has the characteristic of high resolution. The method of the present invention is aimed at environmental barrier coatings, but is not limited to environmental barrier coatings. The method can be used to measure the stress distribution of thermal spray coatings with similar structures and coatings after corrosion, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0030] Figure 1 This is a schematic diagram of the structure of the environmental barrier coating of the present invention;

[0031] Figure 2 Raman spectra of substrate and coating of SiC / Si / Yb2Si2O7 coating system;

[0032] Figure 3 Schematic diagram of SiC substrate tensile test;

[0033] Figure 4 Raman spectra at different positions of the stretched silicon carbide sample;

[0034] Figure 5 is the Raman frequency shift and frequency shift ratio diagram of SiC and Si;

[0035] Figure 6 The Raman frequency shift and frequency shift ratio diagram of Si and Yb2Si2O7;

[0036] Figure 7 This is the stress distribution diagram of Si / Yb2Si2O7;

[0037] Figure 8 The Raman frequency shift and frequency shift ratio diagram of Ca2Yb8(SiO4)6O2 and Yb2Si2O7;

[0038] Fig. 9 This is the stress distribution diagram of Si / Yb2Si2O7 / Ca2Yb8(SiO4)6O2;

[0039] Fig.10 This is a flow chart of a method for testing residual stress distribution inside an environmental barrier coating according to an embodiment of the present invention. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0042] Embodiment 1:

[0043] like Figure 1 and 10 As shown, an embodiment of the present invention provides a method for testing the internal residual stress distribution of an environmental barrier coating, comprising:

[0044] Step S1, measuring the Raman frequency shift-stress factor of the substrate in the environmental barrier coating by a tensile method, and calibrating the Raman frequency shift-stress factor of each coating layer by layer in situ; the environmental barrier coating system comprises a substrate, a bonding layer and an environmental barrier coating; the substrate material is a silicon carbide fiber reinforced silicon carbide composite material or a silicon nitride fiber reinforced silicon nitride composite material; the bonding layer is a silicon bonding layer or a hafnium oxide modified silicon bonding layer; the environmental barrier coating is a rare earth silicate coating or a corroded rare earth silicate coating.

[0045] Step S2: determining the residual stress state of the test area according to the Raman frequency shift-stress factor and based on the linear relationship between the coating Raman signal and the Raman frequency shift.

[0046] Embodiment 2:

[0047] An embodiment of the present invention provides a method for testing residual stress distribution inside an environmental barrier coating, comprising:

[0048] (21) Calibrate the Raman peak of the coating material in a stress-free state, perform Raman testing on the stress-free state of the substrate and coating material used to prepare the coating, and calibrate the main peak position of the obtained Raman spectrum as the initial Raman absorption peak wave number ω0 of the coating material.

[0049] (22) In the environmental barrier coating system, the coating is too thin to be measured by conventional tensile method. However, the substrate fiber generally meets the tensile measurement requirements. The Raman frequency shift-stress factor R of the substrate is measured by tensile method. E :

[0050]

[0051] Where F is the tensile force on the substrate, S is the stretched cross-sectional area, Δω E =ω E -ω E0 It represents the frequency shift between the actual Raman absorption peak wavenumber of the matrix and the standard absorption peak wavenumber.

[0052] (23) After cold cutting and polishing, the coating to be tested is subjected to smooth cross-sectioning, with a surface roughness of less than 0.15 μm. The coating cross-section is imaged by a microscope system to select the area to be tested.

[0053] (24) According to the accuracy requirements, the Raman signal acquisition step size is set to 1-50 μm. A micro Raman spectrometer is used to collect Raman signals of the stress distribution area to be measured. The minimum laser beam spot diameter of the Raman signal acquisition is less than 1 μm.

[0054] (25) The coating material is a polycrystalline ceramic system. The residual stress measurement adopts a quantitative method that ignores the crystal orientation of the material. After simplifying the stress state, the quantitative stress-frequency shift relationship of the i-th coating layer is:

[0055] σ i =R i (ω i -ω i0 )

[0056] In the collected Raman data, the interface between substrate and coating is selected. The Raman spectra of materials A and B on both sides of the interface are included on the interface between coating and coating. The stress magnitude at the same position is the same, so there is the following relationship:

[0057] σ A =σ B

[0058] The Raman spectrum is fitted and the frequency shift Δω=ω-ω0 between the actual Raman absorption peak wavenumber of each component and the standard absorption peak wavenumber is calculated.

[0059]

[0060] (26) According to the Raman frequency shift-stress factor R of the substrate obtained in (22) E Calculate the Raman frequency shift-stress factor R1 of the adjacent bonding layer, calculate the Raman frequency shift-stress factor R2 of the adjacent coating based on the Raman frequency shift-stress factor of the bonding layer, and calculate the Raman frequency shift-stress factor R of the i-th coating layer. i .

[0061] (27) According to the collected Raman signals of the area to be measured, the Raman frequency shift Δω of each layer and each collection point is calculated. i =ω i -ω i0 , according to the Raman frequency shift-stress factor R of each layer of material obtained in (26) i Then, by the formula:

[0062] σ i =R i (ω i -ω i0 )

[0063] The stress state σ of each test point is calculated i, where the stress states of the boundary points are the same, so just select one of the materials to calculate the stress state.

[0064] (28) The stress state of each test point is imaged to obtain the quantitative result of the stress distribution at the corresponding position of the test area.

[0065] Embodiment 3:

[0066] The embodiment of the present invention measures the residual stress in the SiC / Si / Yb2Si2O7 coating environmental barrier coating system, and the specific steps are as follows:

[0067] (31) Figure 2 As shown in the figure, the Raman spectra of SiC, Si, and Yb2Si2O7 in the stress-free state of the SiC / Si / Yb2Si2O7 coating system were measured, the obtained Raman spectra were peaked and the initial Raman absorption peak wave number ω0 was calibrated. The characteristic peak of SiC was calibrated to 785.15 cm -1 , the characteristic peak of Si is 520.6cm -1 , the characteristic peak of Yb2Si2O7 is 922.25cm -1 , the characteristic peak of Yb2SiO5 is 890.47cm -1 ,.

[0068] (32) In the environmental barrier coating system, since the coating is relatively thin, it is not suitable to directly measure its Raman frequency shift-stress factor by conventional tensile method. However, the Raman frequency shift-stress factor R of the silicon carbide substrate material is E It can be measured by tensile method, such as Figure 3 As shown, the cross-sectional area is cut to 1mm 2 Silicon carbide substrate, stretched with a tensile force of 100N, according to Figure 4 As shown, the measured Raman average shift is 0.31 cm -1 :

[0069]

[0070] The Raman frequency shift-stress factor R of the silicon carbide substrate material was measured. E -322.58MPa / cm -1 .

[0071] (33) After the SiC / Si / Yb2Si2O7 coating to be tested is cold-mounted and cut, a smooth cross section is obtained by polishing. The coating cross section is imaged by a microscope system, and the area of ​​stress distribution to be tested is selected.

[0072] (34) Set the Raman signal acquisition step size to 1 μm, and use a micro-Raman spectrometer to collect Raman signals from the stress distribution area to be measured.

[0073] (35) Raman frequency shift-stress factor R of Si layer Si Perform in-situ calibration and calculate based on the Raman shift of silicon carbide and Si at the same point of the coating:

[0074]

[0075] according to Figure 5 The Raman frequency shift and frequency shift ratio of SiC and Si are plotted, and R is calculated. Si / R Si is 1.60, and the R Si -201.4MPa / cm -1 .

[0076] Similarly, according to Figure 6 The Raman frequency shift and frequency shift ratio diagram of Si and Yb2Si2O7 is calculated to obtain R Yb2Si2O7 / R Si is 3.50, R Yb2Si2O7 -57.5MPa / cm -1 .

[0077] (36) Calculate the Raman frequency shift Δω of each acquisition point in each layer based on the collected Raman signal of the area to be measured i =ω i -ω i0 , according to the Raman frequency shift-stress factor R of each layer of material obtained in (35) i Then, by the formula:

[0078] σ i =R i (ω i -ω i0 )

[0079] The stress state σ of each test point is calculated i , where the boundary points have the same stress state, and the internal stress of Si is selected for calculation at the interface between Si and Yb2Si2O7.

[0080] (37) Obtain the stress state of each test point, process the data and obtain the quantitative imaging result of the stress at the corresponding position of the test area. Figure 7 As shown, the stress state of each point after imaging can be determined by the positive and negative signs of the numerical results after quantification, with a positive sign representing tensile stress and a negative sign representing compressive stress.

[0081] Example 4

[0082] The embodiment of the present invention measures the residual stress of the coating and the corrosion product layer in the SiC / Si / Yb2Si2O7 coating environmental barrier coating system after CMAS corrosion, and the specific steps are as follows:

[0083] (41-44) and steps (31-34) in Example 3 are the same.

[0084] (45) Compared with Example 2, except for the Raman frequency shift-stress factor R of the Si layer, Si and the stress factor R of the Raman shift of Yb2Si2O7 Yb2Si2O7 Outside, through Figure 8 The stress factor R of the Raman shift of the corrosion product Ca2Yb8(SiO4)6O2 was calculated. CP Yes, R CP -91.0MPa / cm -1 .

[0085] (46) Process the collected Raman signals of the area to be measured, and calculate the Raman frequency shift Δω of each layer and each collection point i =ω i -ω i0 , according to the Raman frequency shift-stress factor R of each layer of material obtained in (45) i Then, by the formula:

[0086] σ i =R i (ω i -ω i0 )

[0087] The stress state σ of each test point is calculated i , where the boundary points have the same stress state, and the internal stress of Yb2Si2O7 is selected for calculation at the interface between Ca2Yb8(SiO4)6O2 and Yb2Si2O7.

[0088] (47) The stress state of each test point is obtained, and the quantitative imaging result of the stress at the corresponding position of the test area is obtained by data processing imaging. Fig. 9 As shown, the stress state of each point after imaging can be determined by the positive and negative signs of the numerical results after quantification, with a positive sign representing tensile stress and a negative sign representing compressive stress.

[0089] The embodiments described above are only descriptions of the preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for testing the internal residual stress distribution of an environmental barrier coating, characterized in that: include: Step S1, measuring the Raman frequency shift-stress factor of the substrate in the environmental barrier coating by a tensile method, and calibrating the Raman frequency shift-stress factor of each coating layer by layer in situ; Step S2: determining the residual stress state of the test area according to the Raman frequency shift-stress factor and based on the linear relationship between the coating Raman signal and the Raman frequency shift.

2. The method for testing residual stress distribution inside an environmental barrier coating according to claim 1, characterized in that: The environmental barrier coating system comprises a substrate, a bonding layer and an environmental barrier coating; the substrate material is silicon carbide and its composite material, silicon nitride and its composite material; the bonding layer is silicon and its modified material; Environmental barrier coatings are rare earth silicates or related materials after corrosion.

3. A method for testing the internal residual stress distribution of an environmental barrier coating, characterized in that: include Obtain the initial Raman absorption peak wave number ω0 of the environmental barrier coating material in a stress-free state; Measurement of Raman frequency shift-stress factor R of substrate by stretching method E : After cold cutting and polishing, the coating to be tested is cut to obtain a smooth cross section, and the coating cross section is imaged by a microscope system to select the area to be tested; Use a micro-Raman spectrometer to collect Raman signals from the stress distribution area to be tested; According to the Raman frequency shift of the substrate-stress factor R E Calculate the Raman frequency shift-stress factor R1 of the adjacent bonding layer, calculate the Raman frequency shift-stress factor R2 of the adjacent coating based on the Raman frequency shift-stress factor of the bonding layer, and calculate the Raman frequency shift-stress factor R of the i-th coating layer. i ; According to the Raman signal collected in the test area and the initial Raman absorption peak wave number ω0, the Raman frequency shift Δω of each acquisition point in each layer is calculated. i ; According to the Raman frequency shift of each layer of material-stress factor R i and the Raman frequency shift Δω i , calculate the stress state of each test point; The stress state of each test point is imaged to obtain the quantitative results of the stress distribution at the corresponding position of the test area.

4. The method for testing residual stress distribution inside an environmental barrier coating according to claim 3, characterized in that: The environmental barrier coating system comprises a substrate, a bonding layer and an environmental barrier coating; the substrate material is silicon carbide and its composite material, silicon nitride and its composite material; the bonding layer is silicon and its modified material; Environmental barrier coatings are rare earth silicates or related materials after corrosion.

5. The method for testing residual stress distribution inside an environmental barrier coating according to claim 4, characterized in that: Measure the Raman frequency shift of the substrate - stress factor R E as follows: Where F is the tensile force on the substrate, S is the stretched cross-sectional area, Δω E =ω E -ω E0 It represents the frequency shift between the actual Raman absorption peak wavenumber of the matrix and the standard absorption peak wavenumber.

6. The method for testing residual stress distribution inside an environmental barrier coating according to claim 5, characterized in that: According to the Raman frequency shift of each layer of material-stress factor R i , the stress state of each test point is calculated, s i =R i (oh i -oh i0 ) 7. The method for testing residual stress distribution inside an environmental barrier coating according to claim 6, characterized in that: The stress state of each point after imaging is determined by the positive and negative signs of the numerical results after quantification, with a positive sign indicating tensile stress and a negative sign indicating compressive stress.

8. The method for testing residual stress distribution inside an environmental barrier coating according to claim 7, characterized in that: The minimum laser beam spot diameter for Raman signal collection is less than 1 μm.

Citation Information

Cited By

  • Quantitative characterization method of residual stress and bonding stress amplification structure thereof