Metallographic corrosive agent and corrosion method for delta-ferrite in martensitic stainless steel

By using a mixed solution of oxalic acid, hydrofluoric acid and potassium permanganate to corrode martensite stainless steel at room temperature, the martensite interference problem in δ-ferrite detection in the prior art was solved, and efficient and accurate δ-ferrite content detection, suitable for industrial applications.

CN118913847APending Publication Date: 2024-11-08AVIC STANDARD PARTS MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410856036.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When detecting the δ-ferrite content in martensite stainless steel, the corrosion agent will simultaneously highlight the martensite structure, resulting in measurement interference and errors. The operation is complex and harmful, making it difficult to accurately control δ-ferrite. content.

Method used

Using a mixed solution of oxalic acid, hydrofluoric acid and potassium permanganate as metallurgical corrosive agent, by corroding martensite stainless steel samples at room temperature, only δ-ferrite is highlighted, martensite interference is eliminated, and detection accuracy is improved. Simple and safe operation.

Benefits of technology

Accurate detection of δ-ferrite content is achieved, interference is reduced, and the accuracy of detection results is improved. It is simple and safe to operate, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913847A_ABST
    Figure CN118913847A_ABST
Patent Text Reader

Abstract

A metallographic corrosive agent for delta-ferrite in martensitic stainless steel is characterized by comprising, by weight, 20-40 g of oxalic acid, 5-10 mL of hydrofluoric acid, 1-2 g of potassium permanganate and 90-110 mL of deionized water. The corrosion method comprises the following steps that firstly, 90 mL to 110 mL of deionized water is taken and placed in a beaker, 20 g to 40 g of oxalic acid is weighed and added into the deionized water, stirring is conducted through a glass rod to enable the oxalic acid to be fully dissolved, then 5 mL to 10 mL of hydrofluoric acid is added, stirring continues to be conducted for dissolution, finally 1 g to 2 g of potassium permanganate is added, stirring is conducted till the potassium permanganate is fully dissolved, and manufacturing of the metallographic phase corrosive agent is achieved; secondly, a metallographic sample is obtained through cold inlaying, coarse grinding, accurate grinding and polishing; and 3, immersing a metallographic sample into the prepared corrosive agent, corroding for 60-180 seconds at normal temperature, then cleaning with absolute ethyl alcohol, and drying to obtain a to-be-detected metallographic sample. The method is easy to operate, good in effect, efficient, reliable and suitable for application and popularization of delta-ferrite corrosion in martensitic stainless steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallographic detection of metal materials, and in particular relates to a metallographic corrosive agent and a corrosive method for delta-ferrite in martensitic stainless steel. Background Art

[0002] As one of the important means of metal material testing and research, metallographic testing is to obtain and analyze the microstructure state and distribution with the help of a metallographic microscope, and then explore the quality of metal materials. Among them, the metallographic corrosion process is an essential link, which plays an important role in clearly displaying the microstructure of metal materials.

[0003] Martensite is a common organization name of ferrous metal materials, which is a supersaturated solid solution of carbon in α-Fe. In order to make martensitic stainless steel obtain good comprehensive properties, some alloying elements are often added to widen the austenitization temperature range, reduce the austenite single-phase area, and reduce the ferrite transformation temperature, which makes it very easy for the material to generate δ-ferrite during the production process. The content of δ-ferrite is closely related to the heating temperature. Taking the martensitic-ferritic stainless steel 1Cr17Ni2 as an example, when the heating temperature is 800℃-1000℃, as the heating temperature increases, the content of austenite in its organization increases, and the content of δ-ferrite decreases. When the heating temperature is higher than 1000℃, as the heating temperature increases, the content of austenite in its organization decreases, and the content of δ-ferrite increases. However, a large number of studies have found that a high content of δ-ferrite will increase the strength, hardness, and surface notch sensitivity of the workpiece, reduce plasticity and impact toughness, and easily cause brittle fracture during use. Therefore, the heating temperature should be strictly controlled during the production process to avoid the appearance of excessive δ-ferrite. Therefore, how to accurately detect the δ-ferrite content is crucial.

[0004] At present, many methods for corrosion of δ-ferrite are electrolysis and hot corrosion. Patent CN112730004B discloses a metallographic corrosion method for δ-ferrite of 1Cr13 martensitic stainless steel. The electrolysis method used in the patent uses a mixed solution of perchloric acid and glacial acetic acid as the electrolyte. Patent CN112730003B discloses a metallographic corrosion method for δ-ferrite in 2Cr13 martensitic stainless steel continuous casting billets. The electrolysis method used in the patent uses a mixed solution of perchloric acid and glacial acetic acid as the electrolyte. Patent CN114018920A discloses a method for corrosion of δ-ferrite in P91 and P92 steels. The hot corrosion method is used in the patent and the corrosive agent is an aqueous solution of picric acid.

[0005] In existing patents, most stainless steel corrosive agents will not only highlight δ-ferrite, but also martensite after corrosion. When using the binary extraction method to determine the δ-ferrite content, the highlighted martensite structure will cause certain interference to the measurement, increase the detection workload, and also bring errors to the determination result of the δ-ferrite content. The operation process is complicated, and the corrosive agents used are harmful to a certain extent. Summary of the invention

[0006] The object of the present invention is to overcome the above disadvantages and provide a metallographic etching agent and etching method for delta-ferrite in martensitic stainless steel which is simple to operate, has good effect, is efficient and reliable.

[0007] The purpose of the present invention and the solution of its main technical problems are achieved by adopting the following technical solutions: The metallographic etching agent for delta-ferrite in martensitic stainless steel of the present invention is characterized by comprising, in parts by weight: Oxalic acid 20g-40g, hydrofluoric acid 5mL-10mL, potassium permanganate 1g-2g, deionized water 90mL-110mL.

[0008] The metallographic corrosion method for delta-ferrite in martensitic stainless steel is characterized by comprising the following steps: 1) Preparation of metallographic etchant: Take 90mL-110mL of deionized water and place it in a beaker, weigh 20g-40g of oxalic acid and add it to the deionized water, stir with a glass rod to fully dissolve it, then add 5mL-10mL of hydrofluoric acid, continue stirring to dissolve, and finally add 1g-2g of potassium permanganate and stir until fully dissolved; 2) Metallographic sample preparation: Cut the martensitic stainless steel material according to the product requirements, and cold mount the original sample, and then use 120#-600# sandpaper for rough grinding and 1500#-2500# sandpaper for fine grinding, and use 2.5μm diamond polishing agent to polish for 2min-3min, rinse the sample with water and wipe with alcohol to remove the polishing agent remaining on the surface of the sample, and dry it for use; 3) Corrosion: Immerse the metallographic sample obtained in step 2) in the corrosive agent prepared in step 1), corrode for 60s-180s at room temperature, then clean with anhydrous ethanol and blow dry to obtain a metallographic sample to be tested.

[0009] In the above-mentioned metallographic corrosive agent and corrosion method for delta-ferrite in martensitic stainless steel, the mass concentration of the oxalic acid is ≥99.5%.

[0010] In the above-mentioned metallographic corrosive agent and corrosion method for delta-ferrite in martensitic stainless steel, the volume concentration of the hydrofluoric acid is ≥40%.

[0011] In the above-mentioned metallographic corrosive agent and corrosion method for delta-ferrite in martensitic stainless steel, the mass concentration of the potassium permanganate is ≥99.5%.

[0012] Compared with the prior art, the present invention has obvious advantages and beneficial effects. It can be seen from the above technical scheme that in the metallographic etching agent and etching method of δ-ferrite in martensitic stainless steel of the present invention, the metallographic corrosion of δ-ferrite is achieved by making the metallographic etching agent, metallographic sample preparation and corrosion, and only δ-ferrite is highlighted without martensite, which eliminates interference for the calibration of δ-ferrite content, improves the accuracy of the content determination results, better guides production, and provides heat treatment temperatures that meet production requirements. Secondly, the etching agent proposed by the present invention is relatively safe, simple to operate, and does not require electrolysis or heating. In short, the present invention is simple to operate, has good effects, is efficient and reliable, and is suitable for the promotion and use of δ-ferrite corrosion in martensitic stainless steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 Schematic diagram of the microstructure of Example 1 of the present invention; Figure 2 for Figure 1 Schematic diagram of the microstructure after partial enlargement; Figure 3 Schematic diagram of the microstructure of Example 2 of the present invention; Figure 4 for Figure 3 Schematic diagram of the microstructure after partial enlargement; Figure 5 Schematic diagram of the microstructure of Example 3 of the present invention; Figure 6 for Figure 5 Schematic diagram of the microstructure after partial enlargement; Figure 7 Schematic diagram of the microstructure of conventional etchant comparative example 4; Figure 8 for Figure 7 Schematic diagram of the microstructure after local enlargement. DETAILED DESCRIPTION

[0014] In conjunction with the accompanying drawings and preferred embodiments, the specific implementation manner, structure, characteristics and efficacy of a metallographic etching agent and etching method for delta-ferrite in martensitic stainless steel proposed in accordance with the present invention are described in detail below.

[0015] The nut made of 1Cr17Ni2 material was subjected to solution aging treatment, and Examples 1-3 were carried out using the corrosive agent of the present invention, and Comparative Example 4 was carried out using a conventional corrosive agent, and the structure was observed and analyzed through an optical microscope.

[0016] Embodiment 1: A metallographic corrosion method for delta-ferrite in martensitic stainless steel comprises the following steps: 1) Preparation of metallographic etchant: Take 90mL of deionized water and place it in a beaker, weigh 20g of oxalic acid with a mass concentration of 99.5% and add it to the deionized water, stir with a glass rod to fully dissolve it, then add 10mL of hydrofluoric acid with a volume concentration of 40%, continue stirring to dissolve, and finally add 2g of potassium permanganate with a mass concentration of 99.5% and stir until it is fully dissolved; 2) Metallographic sample preparation: The martensitic stainless steel material is cut according to the product requirements, and the original sample is cold mounted, and then coarsely ground with 120# and 600# sandpaper, finely ground with 1500# sandpaper, and polished with 2.5μm diamond polishing agent for 3 minutes. The sample is rinsed with water and wiped with alcohol to remove the polishing agent remaining on the surface of the sample, and then dried for use; 3) Corrosion: The metallographic sample obtained in step 2) is immersed in the corrosive agent prepared in step 1), corroded at room temperature for 180 seconds, and then cleaned with anhydrous ethanol and blown dry to obtain a metallographic sample to be tested.

[0017] Embodiment 2: A metallographic corrosion method for delta-ferrite in martensitic stainless steel comprises the following steps: 1) Preparation of metallographic etchant: Take 100mL of deionized water and place it in a beaker, weigh 30g of oxalic acid with a mass concentration of 99.5% and add it to the deionized water, stir with a glass rod to fully dissolve it, then add 10mL of hydrofluoric acid with a volume concentration of 40%, continue to stir and dissolve it, and finally add 2g of potassium permanganate with a mass concentration of 99.5% and stir until it is fully dissolved; 2) Metallographic sample preparation: The martensitic stainless steel material is cut according to the product requirements, and the original sample is cold mounted, and then coarsely ground with 120# and 600# sandpaper, and finely ground with 1500# and 2000# sandpaper. A 2.5μm diamond polishing agent is used for polishing for 2.5min. The sample is rinsed with water and wiped with alcohol to remove the polishing agent remaining on the surface of the sample, and then dried for use; 3) Corrosion: The metallographic sample obtained in step 2) is immersed in the corrosive agent prepared in step 1), corroded at room temperature for 60 seconds, and then cleaned with anhydrous ethanol and blown dry to obtain a metallographic sample to be tested.

[0018] Embodiment 3: A metallographic corrosion method for delta-ferrite in martensitic stainless steel comprises the following steps: 1) Preparation of metallographic etchant: Take 110mL of deionized water and place it in a beaker, weigh 40g of oxalic acid with a mass concentration of 99.5% and add it to the deionized water, stir with a glass rod to fully dissolve it, then add 5mL of hydrofluoric acid with a volume concentration of 40%, continue stirring to dissolve, and finally add 1g of potassium permanganate with a mass concentration of 99.5% and stir until it is fully dissolved; 2) Metallographic sample preparation: The martensitic stainless steel material is cut according to the product requirements, and the original sample is cold mounted, and then coarsely ground with 120# and 600# sandpaper, and finely ground with 1500# and 2500# sandpaper. 2.5μm diamond polishing agent is used for polishing for 2 minutes. The sample is rinsed with water and wiped with alcohol to remove the polishing agent remaining on the surface of the sample, and then dried for use; 3) Corrosion: The metallographic sample obtained in step 2) is immersed in the corrosive agent prepared in step 1), corroded at room temperature for 120 seconds, and then cleaned with anhydrous ethanol and blown dry to obtain a metallographic sample to be tested.

[0019] Conventional Corrosive Agent Comparative Example 4: A metallographic corrosion method for delta-ferrite in martensitic stainless steel comprises the following steps: 1) Preparation of metallographic etchant: Take 90mL of deionized water and place it in a beaker, take 3g of ferric chloride and pour it into the beaker, stir with a glass rod to fully dissolve it, then add 10ml of hydrochloric acid, stir with a glass rod, and let it stand; 2) Metallographic sample preparation: The martensitic stainless steel material is cut according to the product requirements, and the original sample is cold mounted, and then coarsely ground with 120# and 600# sandpaper, and finely ground with 1500# and 2000# sandpaper. A 2.5μm diamond polishing agent is used for polishing for 2.5min. The sample is rinsed with water and wiped with alcohol to remove the polishing agent remaining on the surface of the sample, and then dried for use; 3) Corrosion: The metallographic sample obtained in step 2) is immersed in the corrosive agent prepared in step 1), corroded at room temperature for 20 seconds, and then cleaned with anhydrous ethanol and blown dry to obtain a metallographic sample to be tested.

[0020] By observation Figure 1-Figure 6 , and found that compared with Figure 7 and Figure 8 In Examples 1-3, prominent δ-ferrite can be clearly observed, and no martensite is found, which eliminates interference in the calibration of the δ-ferrite content and improves the accuracy of the content determination results.

[0021] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A metallographic etchant for delta-ferrite in martensitic stainless steel, characterized in that: By weight ratio: Oxalic acid 20g-40g, hydrofluoric acid 5mL-10mL, potassium permanganate 1g-2g, deionized water 90mL-110mL.

2. A metallographic corrosion method for delta-ferrite in martensitic stainless steel, characterized in that: The following steps are involved: 1) Preparation of metallographic etchant: Take 90mL-110mL of deionized water and place it in a beaker, weigh 20g-40g of oxalic acid and add it to the deionized water, stir with a glass rod to fully dissolve it, then add 5mL-10mL of hydrofluoric acid, continue stirring to dissolve, and finally add 1g-2g of potassium permanganate and stir until fully dissolved; 2) Metallographic sample preparation: Cut the martensitic stainless steel material according to the product requirements, and cold mount the original sample, and then use 120#-600# sandpaper for rough grinding and 1500#-2500# sandpaper for fine grinding, and use 2.5μm diamond polishing agent to polish for 2min-3min, rinse the sample with water and wipe with alcohol to remove the polishing agent remaining on the surface of the sample, and dry it for use; 3) Corrosion: Immerse the metallographic sample obtained in step 2) in the corrosive agent prepared in step 1), corrode for 60s-180s at room temperature, then clean with anhydrous ethanol and blow dry to obtain a metallographic sample to be tested.

3. The metallographic etching agent and etching method for delta-ferrite in martensitic stainless steel according to claim 1, characterized in that: The mass concentration of the oxalic acid is ≥99.5%.

4. A metallographic etchant and etching method for delta-ferrite in martensitic stainless steel as claimed in claim 1, characterized in that: The volume concentration of the hydrofluoric acid is ≥40%.

5. The metallographic etching agent and etching method for delta-ferrite in martensitic stainless steel according to claim 1, characterized in that: The mass concentration of the potassium permanganate is ≥99.5%.