Method and device for dynamically detecting volume change rate of elastomer sealing element
Through the built-in balance measuring the floating weight change, combined with Archimedes theorem to calculate the volume change rate, the problems of low detection accuracy and corrosion ease in the existing technology are solved, and the real-time elastomer seals are realized in high temperature and high pressure environment. Accurate volume change monitoring, simplifying operation and reducing corrosion risks.
Patent Information
- Application Number
- CN202310505054.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art detects the volume change rate of elastomeric seals during corrosion of high temperature and high pressure CO2, and the detection device is vulnerable to corrosion.
Using a dynamic detection method with built-in balance, by measuring the floating and weight change of the sample in solution, and combining Archimedes theorem to calculate the volume change rate, it provides a method and device for dynamic detection of the volume change rate of elastomer seal, including protection The layer, reactor, heating temperature measuring device and built-in balance ensure measurement accuracy and stability.
Real-time and accurate detection of volume changes of elastomeric seals in high temperature and high pressure environments is achieved, which avoids errors and reduces the corrosion risk of the detection device, and simplifies the operation process.
Smart Images

Figure CN118913997A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to oil and gas field CO 2 The technical field of corrosion evaluation relates to a method and device for dynamically detecting the volume change rate of an elastomeric seal. Background Art
[0002] CCUS-EOR is a process that converts the collected CO 2 Inject into the oil layer to allow CO 2 It is soluble in crude oil, causing the volume of crude oil to expand, viscosity to decrease, interfacial tension to decrease, and fluidity to increase, thereby achieving the purpose of increasing crude oil recovery. This method can also make a large amount of industrial CO 2 Buried underground, it plays a role in reducing greenhouse gas emissions. However, during the gas injection process, CO 2 When the content increases significantly, the CO resistance of underground facilities 2 The corrosion problem is an issue that must be focused on. For metal materials such as steel, their CO resistance can be improved by adding corrosion-resistant alloys, coatings, etc. 2 However, for elastomer seals, how to improve their resistance to CO2 in high temperature and high pressure environments? 2 The corrosion problem needs to be solved urgently. For example, the packer rubber is a very important rubber product that plays a sealing role in oil field mining operations. Once corrosion occurs, it will affect its sealing performance, thereby causing oil and gas well production safety. To address this problem, on the one hand, the corrosion resistance of the product can be improved by modifying the material of the product; on the other hand, for rubber and other elastomers in CO 2 Real-time and effective detection and evaluation of corrosion in gas injection wellbore conditions is also particularly important to avoid safety problems caused by corrosion.
[0003] The corrosion of elastomers is mainly due to H 2 O、N 2 , CO 2 When small molecules enter the elastomer, the bonds are destroyed, resulting in bubbling and cracking. During the corrosion process, the bubbling and cracking of the elastomer will bring about changes in mass and volume. Therefore, the changes in mass and volume of the elastomer are the most direct and important reference indicators for quantitatively evaluating its corrosion resistance.
[0004] At present, the volume change of elastomers before and after corrosion is usually measured by the water displacement method. However, after the experiment, the solution will adhere to the surface of the sample or the cracks. If the water is directly wiped away, there will be a large error; further drying will greatly extend the test time; in addition, for materials with small volume changes, the use of the water displacement method may lead to large errors due to its low accuracy.
[0005] In addition, there is another method, that is, installing a camera in the reactor to achieve real-time monitoring of changes in the reactor. Chinese invention patent CN217140338U discloses a new antioxidant reactor with a camera function. This method has a built-in camera at the top of the reactor and connects it to the monitor in the main control room, which realizes real-time monitoring of the reaction process in the reactor. However, the monitoring effect is limited for corrosion phenomena such as the initial stage of corrosion where changes are not obvious. In addition, high-definition cameras are expensive and still have many limitations when used in corrosive environments.
[0006] Chinese invention patent CN217747074U discloses a method for manufacturing a reactor capable of remotely observing internal materials. A camera is fixedly installed on the right side of the top of the inner wall of the reactor body, and a remote observation device is fixedly connected to the rear side of the reactor body. The device uses a camera instead of a transparent plate to observe the inside of the reactor. The camera is also limited by high temperature and corrosive environment.
[0007] Chinese invention patent application CN115560978A discloses a sealing ring swelling test device and method, which can measure the swelling of different temperatures and H in real time. 2 The weight and volume changes of the sealing ring during the swelling process of hydrogen absorption under partial pressure conditions can accurately characterize the swelling of the hydrogen O-ring. The changes in mass and volume require analysis by a complex information processing system, and it is also difficult to measure the sample in the solution. Summary of the invention
[0008] In order to address the deficiencies in the prior art, the present invention provides a method and device for dynamically detecting the volume change rate of an elastomeric seal, which can detect the mass and volume changes of the elastomeric seal in a solution in real time, and reflect the corrosion condition of the elastomeric seal, so as to address the problems of low detection accuracy, inability to directly and quantitatively monitor the degree of elastomer corrosion in a liquid environment, and susceptibility of detection components to corrosion in the prior art.
[0009] During the service of the elastomer seal in the medium, due to the small molecule H 2 O、N 2 , CO 2 When the gas enters the elastomer, it will destroy the cross-linking bonds of the elastomer, causing bubbles on the surface of the elastomer to expand in volume. Because the volume expansion increases the buoyancy of the elastomer in the medium, its buoyancy changes, and the buoyancy measured by the balance decreases; when too much gas enters the elastomer, the bubbles burst, the buoyancy decreases, and the buoyancy of the elastomer increases. Based on this principle, the patent of this invention can understand the volume change of the elastomer seal during the corrosion process of small molecule gases by real-time monitoring of the change in its buoyancy, thereby understanding its corrosion process.
[0010] Specific working principle: According to Archimedes' theorem, any object immersed in a liquid is subject to buoyancy (liquid static pressure), and the magnitude of the buoyancy is equal to the weight of the liquid displaced by the object. Therefore, the formula for the displacement method is as follows:
[0011] M1-M2=ρV
[0012] Wherein, M1 is the dry weight of the sample, i.e., the weight of the sample in the air in a dry state, M2 is the buoyant weight immersed in liquid, ρ is the density of the solution in the reactor, and V is the volume of liquid displaced when the sample is completely immersed in the liquid.
[0013] According to the above principle, the present invention provides a method for dynamically detecting the volume change of an elastomeric seal, comprising the following steps:
[0014] S1: weigh the dry weight of the sample, recorded as M1;
[0015] S2: Immerse the sample in the solution in the reactor, and when it is fully soaked, reset the balance to zero;
[0016] S3: Inject gas medium into the reactor and raise the temperature. After the temperature of the solution in the reactor and the partial pressure of the injected gas are stable, measure the initial floating weight of the sample by the built-in balance, record it as M2, and calculate the volume change △V in this process;
[0017] S4: test time is t n The sample mass is recorded as Mn, and the time t n The volume change △Vn is calculated by the mass change, and the volume change rate is further obtained
[0018] The mass measured by the built-in balance is the mass change of the sample in the solution.
[0019] Furthermore, in step S2, when the sample is immersed in the solution in the reactor, the gas inside the sample is discharged due to the infiltration of the solution, resulting in an increase in the floating weight. When the floating weight recorded by the balance no longer increases, it means that the infiltration is sufficient, and the time is recorded as t 1 .
[0020] Furthermore, in step S3, the time after the temperature of the solution in the reactor and the partial pressure of the injected gas are stabilized is recorded as t 2 ; At this time, the volume change △V 2 Calculated according to the following formula:
[0021]
[0022] Where ρ is the density of the solution in the reactor.
[0023] Furthermore, in step S4, during the test, any test time t nThe volume change △Vn at this time is calculated according to the following formula:
[0024]
[0025] Furthermore, the volume change rate Calculated according to the following formula:
[0026]
[0027] Where V1 is the initial volume of the sample.
[0028] Therefore, the volume change rate According to this formula, the volume change rate of the elastomer seal during the entire experimental period can be obtained.
[0029] Furthermore, in step S2, the solution in the reactor is oil field produced water, deionized water or seawater.
[0030] Furthermore, in step S3, the injected gas medium is CO 2 ; The injected gas partial pressure is 8-30MPa.
[0031] Furthermore, in step S3, the temperature of the solution in the reactor is room temperature-200°C.
[0032] Furthermore, in step S4, the experimental period is 72-240 hours.
[0033] In addition, the present invention also provides a device for dynamically detecting the volume change rate of an elastomeric seal, which is used to implement any of the above methods. The device includes a protective layer, a reactor arranged in the protective layer, a heating and temperature measuring device, an insulating layer and a built-in balance; the outer wall of the reactor is provided with the heating and temperature measuring device; the bottom of the reactor is provided with an insulating layer and a built-in balance in sequence.
[0034] The protective layer includes an outer cylinder and a heat-insulating layer arranged on the inner wall of the outer cylinder, which is used to maintain the temperature in the reactor stable and not be affected by the external environment;
[0035] The top of the reactor was provided with a gas injection port, and CO was injected into the reactor during the experiment. 2 Gas medium; The maximum temperature resistance of the reactor is 200℃; The maximum pressure resistance is 40MPa; CO 2 , H 2 S and acid solution corrosion;
[0036] The heating and temperature measuring device comprises a heating coil and a temperature measuring thermocouple. The outer wall of the reactor is provided with a heating coil to provide a heat source for the reactor and set the required temperature for the reaction. The temperature measuring thermocouple is connected to the heating coil to test the temperature of the solution in the reactor.
[0037] The heat insulation layer is a heat insulation cotton or a heat insulation board, which is used to ensure that when the temperature in the reactor is ≤200°C, the temperature of the built-in balance is ≤30°C, so as to ensure that the test accuracy and numerical stability of the built-in balance are not affected by the temperature change in the reactor;
[0038] The built-in balance can measure and display the mass change of the sample in the reactor in real time;
[0039] The built-in balance has an accuracy of ≥0.001g and a measuring range of ≥20kg, and is used to accurately measure the change in the floating weight of the sample in the solution in the reactor.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] (1) Beneficial effects of the detection method:
[0042] 1. Compared with the drainage method used in the prior art, the use of a balance with an accuracy of ≥0.001g can detect and record in real time the changes in the floating weight of the sample in the reactor solution caused by the entry of small molecules into the elastomer seal, and the results are more accurate; and the detection process does not require drying and other steps, making the operation simpler;
[0043] 2. Compared with the prior art method of installing a camera in the device, the method of the present invention can realize real-time quantitative detection and accurately reflect the corrosion process of the sample during the experimental period through the quantitative index of volume change rate;
[0044] 3. By using a built-in balance to detect the change in the floating weight of the sample in the solution and then obtain the volume change, the problem that the existing technology cannot directly test the mass and volume of the sample in the solution is solved.
[0045] (2) Beneficial effects of the detection device:
[0046] 1. The reaction device is equipped with a built-in balance for real-time dynamic detection, without manual monitoring, and simple operation; the balance is placed outside the reactor and is not easily corroded by the solution or gas in the reactor;
[0047] 2. The balance accuracy used in the reaction device is ≥0.001g, which can accurately measure the floating weight change caused by the slight volume change of the sample;
[0048] 3. An insulation layer is set between the reactor and the built-in balance to effectively block the temperature changes caused by heat diffusion in the reactor, so that when the temperature in the reactor is ≤200℃, the temperature of the balance is ≤30℃, to ensure that the test accuracy and numerical stability of the built-in balance are not affected by the temperature changes in the reactor. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1Schematic diagram of the device structure for detecting the volume change rate of elastomeric seals.
[0050] Markings in the figure: 1—protective layer; the protective layer also includes: 101—outer cylinder, 102—insulating layer arranged on the inner wall of the outer cylinder; 2—heating and temperature measuring device; 3—reactor arranged in the protective layer; 4—insulating layer; 5—built-in balance; 6—sample to be tested.
[0051] In the present invention, all drawings are schematic drawings, which are only used to illustrate the principles of the present invention and are not drawn according to the actual scale. DETAILED DESCRIPTION
[0052] Each embodiment of the present invention uses a rubber cartridge as a test sample, and tests the 2 Detect the test cartridge in CO under different gas partial pressure and liquid conditions. 2 The mass and volume changes during the corrosion process are described in detail. 2 Corrosion blister cracking test method and apparatus.
[0053] Example 1
[0054] This embodiment provides a method for dynamically detecting the volume change rate of an elastomeric seal, the method comprising the following steps:
[0055] (1) Take the rubber cartridge (according to the working conditions, the volume V1 is 80cm 3 , mass M1 is 100.000g) as the experimental object, weigh the dry weight of the rubber cartridge, record it as M1;
[0056] (2) Pour the solution into the reactor and immerse the rubber cartridge in the solution. After the rubber cartridge is fully soaked and the solution is still, reset the balance to zero.
[0057] (3) Inject gas medium into the reaction device, increase the temperature, and after the temperature and gas partial pressure are stable, measure and record the initial buoyant weight of the sample using the built-in balance, which is recorded as M2; Calculate the volume change △V in this process 2 ;
[0058] (4) The test process continuously records the changes in sample mass during the entire experimental period. The test time is t n The mass is recorded as Mn, and the volume change of the elastomer seal during the entire experimental period is calculated. The volume change rate of the elastomer seal during the entire experimental period can be obtained.
[0059] Example 2
[0060] This embodiment provides a device for dynamically detecting the volume change rate of an elastomeric seal, which is used to implement the method in Embodiment 1.
[0061] like Figure 1 As shown, the device comprises a protective layer 1 and a reactor 2 arranged in the protective layer; a heating and temperature measuring device 3 is arranged on the outer wall of the reactor; and a heat insulating layer 4 and a built-in balance 5 are arranged in sequence at the bottom of the protective layer.
[0062] Specifically, the protective layer 1 includes an outer cylinder 101 and a heat-insulating layer 102 arranged on the inner wall of the outer cylinder, so as to maintain the temperature in the reactor stable and not be affected by the external environment.
[0063] The reactor 2 is arranged in the insulation layer 102, and a gas injection port is provided on the top of the reactor for injecting CO into the reactor. 2 The reactor has a maximum temperature resistance of 200°C, a maximum pressure resistance of 40MPa, and is resistant to CO 2 , H 2 S and acidic solutions.
[0064] The heating and temperature measuring device 3 includes a heating coil and a temperature measuring thermocouple; the heating coil is sleeved on the outer wall of the reactor 2 to provide a heat source for the reactor and set the required temperature for the reaction; the temperature measuring thermocouple is connected to the heating coil to test the temperature of the solution in the reactor.
[0065] The heat insulation layer 4 and the built-in balance 5 are sequentially arranged at the bottom of the reactor 2. The heat insulation layer 4 is a heat insulation cotton or a heat insulation board, which is used to ensure that when the temperature in the reactor is ≤200°C, the temperature of the balance is ≤30°C, so as to ensure that the test accuracy and numerical stability of the built-in balance are not affected by the temperature change in the reactor; the built-in balance 5 is used to measure and display the mass change of the sample in the reactor in real time, and the accuracy of the built-in balance is ≥0.001g, and the range is ≥20kg.
[0066] Embodiment 3:
[0067] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0068] First, take the test rubber cylinder and weigh its dry weight, which is recorded as M1. Secondly, take the produced water (density 1g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The temperature of the solution in the reactor was set to 80°C. CO was then injected. 2 Gas, CO in reactor 2The partial pressure is 8MPa. After the temperature and gas partial pressure are stable, record the initial mass of the built-in balance recording system, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time. The experimental period is 168h.
[0069] Embodiment 4:
[0070] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0071] Compared with Example 3, the only difference is that the temperature of the solution in the reactor is 120°C;
[0072] First, take the test rubber cylinder and weigh its dry weight, which is recorded as M1. Secondly, take the produced water (density 1g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The temperature of the solution in the reactor was set to 120°C. CO was then injected. 2 Gas, CO in reactor 2 The partial pressure is 8MPa. After the temperature and gas partial pressure are stable, record the initial mass of the built-in balance recording system, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time. The experimental period is 168h.
[0073] Embodiment 5:
[0074] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0075] Compared with Example 3, the only difference is that the temperature of the solution in the reactor is 200°C;
[0076] First, take the test rubber cylinder and weigh its dry weight, which is recorded as M1. Secondly, take the produced water (density 1g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The temperature of the solution in the reactor was set to 200°C. CO was then injected. 2 Gas, CO in reactor 2 The partial pressure is 8MPa. After the temperature and gas partial pressure are stable, record the initial mass of the built-in balance recording system, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time. The experimental period is 168h.
[0077] Embodiment 6:
[0078] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0079] Compared with Example 3, the only difference is that the CO2 The partial pressure is 18MPa;
[0080] First, take the test rubber cylinder and weigh its dry weight, which is recorded as M1. Secondly, take the produced water (density 1g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The reactor temperature was set to 80°C. CO was then injected. 2 Gas, CO in reactor 2 The partial pressure is 18 MPa. After the temperature and gas partial pressure are stable, record the initial mass of the built-in balance recording system, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time. The experimental period is 168 hours.
[0081] Embodiment 7:
[0082] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0083] Compared with Example 3, the only difference is that the CO 2 The partial pressure is 30MPa;
[0084] First, take the test rubber cylinder and weigh its dry weight, which is recorded as M1. Secondly, take the produced water (density 1g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The temperature of the solution in the reactor was set to 80°C. CO was then injected. 2 Gas, CO in reactor 2 The partial pressure is 30MPa. After the temperature and gas partial pressure are stable, record the initial mass of the built-in balance recording system, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time. The experimental period is 168h.
[0085] Embodiment 8:
[0086] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0087] Compared with Example 3, the only difference is that the solution is replaced with deionized water;
[0088] First, take the test cartridge and weigh its dry weight, which is recorded as M1. Then, take deionized water (density 1 g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The temperature of the solution in the reactor was set to 80°C. CO was then injected. 2 Gas, CO in reactor 2The partial pressure is 8 MPa, and the initial mass of the built-in balance recording system is recorded at this time, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time, and the experimental period is 168 hours.
[0089] Embodiment 9:
[0090] The following experiment was carried out using the method in Example 1 and the device in Example 2:
[0091] Compared with Example 3, the only difference is that the solution is replaced by seawater;
[0092] First, take the test rubber cylinder and weigh its dry weight, which is recorded as M1. Then, take seawater (density 1g / cm 3 ) was added to the reactor. After the solution was still, the built-in balance was reset to zero. The cartridge was placed in the reactor and completely immersed in the solution. The reactor temperature was set to 80°C. CO was then injected. 2 Gas, CO in reactor 2 The partial pressure is 8 MPa, and the initial mass of the built-in balance recording system is recorded at this time, that is, the floating weight of the rubber cartridge M2; turn on the balance to weigh and record the mass Mn of the rubber cartridge in the solution in real time, and the experimental period is 168 hours.
[0093] The dry weight of the rubber cartridge in the experimental period of each embodiment of the present invention and the mass after 168 hours of reaction are shown in Table 1. It can be seen from Table 1 that the method and device of the present invention can effectively detect the volume change rate of the elastomer seal in different temperatures, different gas partial pressures and different solutions; and because a heat insulation layer is provided between the built-in balance and the reactor, it is effectively ensured that the built-in balance works in a temperature environment without being affected by the temperature change of the reactor; in addition, the use of a high-precision balance can accurately test the volume change rate of the rubber cartridge in the solution due to small molecule CO 2 Slight change in buoyancy caused by the infiltration of gas.
[0094] Table 1 Record of the mass and volume change rate of the rubber cylinder during the experiment
[0095]
[0096] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A method for dynamically detecting the volume change rate of an elastomeric seal, characterized in that: The following steps are involved: S1: weigh the dry weight of the sample, recorded as M1; S2: Immerse the sample in the solution in the reactor, and when it is fully soaked, reset the balance to zero; S3: Inject gas medium into the reactor and raise the temperature. After the temperature of the solution in the reactor and the partial pressure of the injected gas are stable, measure the initial floating weight of the sample by the built-in balance, record it as M2, and calculate the volume change △V of the sample in this process; S4: test time is t n The sample mass is recorded as Mn, and the time t n The volume change △Vn is calculated by the mass change, and the volume change rate is further obtained 2. The method according to claim 1, characterized in that In step S3, the volume change ΔV is calculated according to the following formula: Where ρ is the density of the solution in the reactor.
3. The method according to claim 1, characterized in that In step S4, the volume change rate Calculated according to the following formula: Where V1 is the initial volume of the sample.
4. The method according to claim 1, characterized in that In step S2, the solution in the reactor is oil field produced water, deionized water or sea water.
5. The method according to claim 1, characterized in that In step S3, the injected gas medium is CO2; and the injected gas partial pressure is 8-30 MPa.
6. The method according to claim 1, characterized in that In step S3, the temperature of the solution in the reaction kettle is room temperature-200°C.
7. The method according to claim 1, characterized in that In step S4, the experimental period is 72-240 hours.
8. A device for dynamically detecting the volume change rate of an elastomeric seal, used to implement the method according to any one of claims 1 to 7, characterized in that: The device comprises a protective layer and a reactor arranged in the protective layer; a heating and temperature measuring device is arranged on the outer wall of the reactor; and a heat insulating layer and a built-in balance are arranged in sequence on the bottom of the reactor.
9. The device according to claim 8, characterized in that The protective layer comprises an outer cylinder and a heat-insulating layer arranged on the inner wall of the outer cylinder.
10. The device according to claim 8, characterized in that A gas injection port is provided on the top of the reactor; the reactor has a maximum temperature resistance of 200°C, a maximum pressure resistance of 40MPa, and is resistant to corrosion by CO2, H2S and acidic solutions.
11. The device according to claim 8, characterized in that The heating and temperature measuring device comprises a heating coil and a temperature measuring thermocouple; the heating coil is sleeved on the outer wall of the reactor; the temperature measuring thermocouple is connected to the heating coil and is used to test the temperature of the solution in the reactor.
12. The device according to claim 8, characterized in that The heat insulation layer is heat insulation cotton or heat insulation board.
13. The device according to claim 8, characterized in that The precision of the built-in balance is ≥0.001g, and the measuring range is ≥20kg.