Accelerated storage test method for aluminized film

Through the accelerated storage test method of aluminum-plated film, the problem of performance degradation of aluminum-plated films during long-term storage is solved. By determining the degradation parameters and designing fixtures, building a degradation model and optimizing the test plan, the performance data acquisition of aluminum-plated films is achieved. Ensure its reliability assessment in the spatial environment.

CN118914053APending Publication Date: 2024-11-08BEIJING TIANYU AEROSPACE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411122395.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The performance degradation of aluminum-plated films during long-term ground storage is difficult to obtain data effectively, and the films are easily damaged during the test, which affects the accuracy of the data.

Method used

A test method for accelerated storage of aluminum-plated thin films was designed. By determining degradation performance parameters, designing fixtures, determining critical temperature stress levels, building degradation models and optimization test schemes, step stress tests and D optimization strategies for maximizing Fisher information matrix were adopted. , ensure the accuracy and reliability of the test data.

Benefits of technology

Effectively obtain accelerated storage data of aluminum-plated films to ensure the accuracy of their reliability assessment in the spatial environment, avoid film damage during the test, and ensure effective acquisition of performance parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118914053A_ABST
    Figure CN118914053A_ABST
Patent Text Reader

Abstract

The invention discloses an accelerated storage test method for an aluminized film, and belongs to the technical field of thermal control materials and accelerated tests. The method comprises the following steps: firstly, determining performance parameters of degradation of the aluminum-plated film under a long-term storage condition; then, determining performance parameter detection equipment, detection steps and detection requirements; designing a test fixture according to detection requirements; then, the critical temperature stress level of the degradation mechanism change of the aluminized film is obtained; designing a test scheme and a stress loading mode; secondly, designing a test scheme and a stress loading mode; and finally, determining test equipment, and carrying out an accelerated storage test of the aluminized film. By means of the method, the consistency of the degradation mechanism of the aluminized film within the test stress range and simulation of the storage state can be guaranteed, and effective development of the ground accelerated storage test of the aluminized film is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal control materials and accelerated tests, and relates to an accelerated storage test method for an aluminum-plated film. Background Art

[0002] Aluminum-coated film is light and dust-free. It is a commonly used flexible passive thermal control material for spacecraft. Its thermal insulation performance directly affects the thermal control effect of spacecraft. After evaluation and verification, the aluminum-coated film directly shipped from the factory meets the life and reliability requirements of the space environment. However, during the entire life cycle, the aluminum-coated film will first be stored on the ground for a long time, and then experience the space environment in space. During the long-term storage stage, the temperature and humidity environment on the ground will cause the performance of the aluminum-coated film to degrade, thereby affecting its reliability in service in the space environment. Domestic aluminum-coated film manufacturers and related research institutions have done a lot of research on its performance changes in the space environment, but there are few reports on its long-term storage capacity under ground temperature and humidity conditions. Therefore, conducting effective ground accelerated storage tests is a key measure to explore the performance changes of aluminum-coated films during storage and ensure their reliable operation in the space environment.

[0003] Although the method of modeling and evaluation based on accelerated storage data is relatively mature, there are the following challenges in obtaining effective accelerated storage data for aluminum-coated films: First, the degradation mechanism of aluminum-coated films is complex. Existing studies have shown that the aluminum compounds produced by aluminum corrosion in high and low temperature environments are different, which affects the corrosion rate of aluminum and, in turn, the performance degradation rate of aluminum-coated films. Blindly increasing temperature stress may change its performance degradation mechanism and undermine the principle of unchanged failure mechanism of accelerated degradation modeling. In addition, aluminum-coated films are different from traditional electromechanical products. They are very light and difficult to maintain their own stability during the test. Surface contact during the test and detection process will scratch the surface of the aluminum-coated film, destroying the accuracy of performance data acquisition. Therefore, how to determine the stress level of accelerated storage, design a fixture to simulate the storage state of the aluminum-coated film, and detect its performance parameters without destroying the product are current technical difficulties. Summary of the invention

[0004] In view of the existing technical difficulties, the present invention proposes an accelerated storage test method for aluminum-coated films, which can effectively obtain accelerated storage data of aluminum-coated films and support long-term storage reliability evaluation of aluminum-coated films.

[0005] The accelerated storage test method of the aluminum-plated film of the present invention comprises the following specific steps:

[0006] The accelerated storage test method for aluminum-plated films has the following specific steps:

[0007] Step 1: Determine the performance parameters of the aluminum film that degrade under storage conditions, including hemispherical emissivity and solar absorptivity.

[0008] Step 2: Determine the testing equipment, testing steps and testing requirements for the performance parameters of the aluminum-plated film described in step 1.

[0009] Step 3: Design the fixture for the aluminum film.

[0010] Step 4: Determine the theoretical critical temperature stress level for the change of the degradation mechanism of the aluminum film as S v .

[0011] Step 5: Determine the actual critical temperature stress level at which the degradation mechanism of the aluminum film changes according to the step stress test method;

[0012] Step 6: Construct a preliminary aluminum film degradation model.

[0013] Step 7: Based on the preliminary degradation model constructed in Step 6 and the actual critical temperature stress level determined in Step 5, design a storage test plan and determine the test stress level.

[0014] In the storage test program design, the stress application range of the test is discretized, and the discretization criterion is:

[0015] (i) According to the critical temperature stress level determined in step 5, set the temperature level range and humidity level range of the test.

[0016] (ii) The selection interval of temperature stress level is 5°C, and the selection interval of humidity stress level is 5%.

[0017] (III) In order to ensure the accuracy of the law exploration, the temperature and humidity at k stress levels should be the same in pairs.

[0018] Based on the above discretization criteria, the D optimization strategy of maximizing the Fisher information matrix is ​​used to obtain the test scheme optimization model. By solving the optimization model, the optimal accelerated storage test scheme is obtained.

[0019] Step 8: Design stress loading method.

[0020] Step 9, determine the test equipment and carry out accelerated storage test of aluminum-plated film.

[0021] After the aluminum-plated film sample is clamped by the fixture designed in step 3, it is placed in a temperature and humidity chamber, and the accelerated storage test of the aluminum-plated film is carried out according to the test plan determined in step 7 and the stress loading method designed in step 8. Before the start of the test, the design plan of step 2 is adopted to test the hemispherical emissivity and solar absorption ratio of each aluminum-plated film sample three times, and the average value is taken as the initial performance value of each sample. Subsequently, every time the detection interval of the performance parameters is reached, all samples are taken out of the temperature and humidity chamber, and the hemispherical emissivity and solar absorption ratio of each sample are tested three times, and the average value is taken and recorded until the test time reaches the deadline.

[0022] The advantages of the present invention are:

[0023] 1. The accelerated storage test method for aluminized film of the present invention designs a test fixture according to the ground storage state and performance parameter test requirements of the aluminized film, thereby ensuring the effective acquisition of the performance parameters of the aluminized film.

[0024] 2. The accelerated storage test method for aluminum-plated films of the present invention obtains the critical temperature stress level at which the degradation mechanism of the aluminum-plated films changes through theoretical analysis and step stress test methods, thereby ensuring the principle of unchanged failure mechanism and the effectiveness of long-term storage reliability evaluation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a flow chart of the accelerated storage test method of aluminum-plated film of the present invention;

[0026] Figure 2 It is a schematic diagram of the design of the aluminum-plated film fixture proposed in the accelerated storage test method of the aluminum-plated film of the present invention;

[0027] Figure 3 It is the stress loading profile in the accelerated storage test method for aluminum-plated films of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0029] The accelerated storage test method of the aluminum-plated film of the present invention is mainly aimed at the following characteristics of the accelerated storage test of the aluminum-plated film:

[0030] (1) As the temperature increases, the compounds produced by aluminum corrosion are different, which affects the corrosion rate of aluminum, and then changes the performance degradation rate of the aluminum-plated film, making the performance degradation of the aluminum-plated film nonlinear with temperature, which destroys the failure mechanism unchanged principle of accelerated degradation modeling;

[0031] (2) Unlike traditional electromechanical products, aluminized films are lightweight and cannot maintain stability under the influence of circulating air in a temperature and humidity chamber. In addition, aluminized films should avoid surface contact during testing and inspection to prevent scratches on the surface and damage to the accuracy of performance data acquisition.

[0032] Based on the above characteristics, the accelerated storage test method of the aluminum-plated film of the present invention determines the effective range of temperature stress and designs a fixture to ensure the fixation and performance detection of the aluminum-plated film, thereby ensuring the effective acquisition of the accelerated storage data of the aluminum-plated film and ensuring the accuracy of the long-term storage reliability evaluation. The specific steps are as follows:

[0033] Step 1: Determine the performance parameters of the aluminum-coated film that degrade under storage conditions.

[0034] For typical aluminized films used in aerospace applications, the hemispherical emissivity reflects the film's radiation capacity relative to a black body, and the solar absorptivity reflects the ratio of the film's absorbed radiation flux to the incident radiation flux. Both the hemispherical emissivity and the solar absorptivity are performance parameters that characterize the thermal control performance of aluminized films, and as the film's performance degrades, the hemispherical emissivity and the solar absorptivity gradually increase.

[0035] Step 2: Determine the performance parameter testing equipment, testing steps and testing requirements for the aluminum-coated film.

[0036] The hemispherical emissivity and solar absorption ratio of the aluminum-plated film performance parameters determined in step 1 are tested using a hemispherical emissivity tester and a spectrophotometer.

[0037] Specifically, the detection steps of hemispherical emissivity are:

[0038] (i) Place the probe of the hemispherical emissivity tester on the gold-plated mirror and black material reference samples, and automatically calibrate the instrument according to the reflected energy;

[0039] (ii) After the calibration is completed, place the aluminum-coated film on the heat sink material table, place the probe of the hemispherical emissivity tester at the center of the aluminum-coated surface of the sample to be tested, and start data testing;

[0040] (III) Wait for 1 minute for the reading to stabilize, then read and record the value;

[0041] The above process is carried out three times, and the arithmetic mean of the three measurement results is taken as the hemispherical emissivity of the measured sample.

[0042] Specifically, the detection steps of solar absorption ratio are as follows:

[0043] (1) Start the spectrophotometer and connect it to the computer. Preheat the equipment for 1 hour.

[0044] (ii) Place the standard white plate in the sample chamber and perform self-calibration of the UV-visible spectrophotometer;

[0045] (iii) After the spectrophotometer self-calibration is completed, remove the standard white plate from the sample chamber;

[0046] (iv) Place the aluminized film into the sample chamber so that the center of the aluminized surface of the sample to be tested faces the spectrophotometer, and close the sample chamber;

[0047] (V) Start the test and record the test results after the test is completed.

[0048] During the above measurement process, according to the detection head test requirements of the hemispherical emissivity tester, the effective measurement surface of the aluminum-coated film should be no less than 55mm in diameter; according to the detection head test height requirements of the spectrophotometer, the aluminum-coated film should be able to be vertically lifted by no less than 20mm from the ground.

[0049] Step 3: Design the fixture for the aluminum film.

[0050] In order to ensure that the aluminized film can be fixed during the test and inspection process, it is necessary to design a fixture for the aluminized film.

[0051] In order to ensure that the clamp can withstand the test requirements of high temperature and high humidity, a 0.25 mm thick white polyethylene plastic is selected to manufacture the clamping surface in this embodiment.

[0052] Further, according to the detection requirements of step 2, in order to meet the requirement that the effective measuring surface is not less than 55mm in diameter, a 70mm*70mm square hole is cut out in the center of the clamping surface; then, two clamping surfaces are manufactured according to the above materials and dimensions; the two clamping surfaces are respectively used as the upper and lower clamping surfaces, and are symmetrically arranged up and down, and the aluminized film is clamped between the two. Considering the long-term micro tensile stress of the aluminized film in the storage state, a high temperature and high humidity resistant tape is used to fix the aluminized film on one of the clamping surfaces, and then the other clamping surface is covered on the sample to be tested, and the two clamping surfaces are bonded by the tape.

[0053] In order to meet the requirement that the film can be vertically lifted to the ground by no less than 20mm, the clamp surface is left 30cm away from the edge of the square hole for connecting the clamp surface support, which is installed on the bottom surface of the lower clamp surface and evenly distributed in the axial direction. In addition, the position reference points are marked on the clamp surface to ensure that the test position is consistent each time as much as possible.

[0054] Step 4: Based on the degradation mechanism of the aluminum-plated film, determine the theoretical critical temperature stress level for the change of the degradation mechanism of the aluminum-plated film.

[0055] Specifically, existing research on aluminum corrosion shows that when the temperature is above 60°C, the compound produced by aluminum corrosion is AlOOH, while the compound produced when the temperature is below 60°C is Al(OH)3. Since AlOOH is more compact than Al(OH)3, the increase in temperature will reduce the rate of aluminum corrosion after exceeding 60°C. In addition, the degradation mechanism of the aluminum-plated film is mainly caused by aluminum corrosion, and the aging of the polymer substrate has little effect on the degradation of the aluminum-plated film. Therefore, the theoretical critical temperature stress level for the change of the degradation mechanism of the aluminum-plated film obtained in the present invention is 60°C.

[0056] Step 5: Determine the actual critical temperature stress level at which the degradation mechanism of the aluminum-plated film changes according to the step stress test method to ensure the consistency of the degradation mechanism within the test stress range.

[0057] According to the theoretical critical temperature stress level of 60℃ determined in step 4, a step temperature stress test is carried out starting from 50℃ with a stress interval of 2℃, and the actual critical temperature stress level S is determined according to the degradation rate of the aluminum film performance. v .

[0058] A 60-hour storage test was conducted at each temperature stress level, in which the performance parameters of the aluminum-plated film were determined once every 12 hours using the method in step 2. A total of 6 performance parameters including the initial performance parameters were collected, and the degradation rate was calculated. If the degradation rate at the current temperature stress level is less than the degradation rate at the previous temperature stress level, the current temperature stress level is the actual critical temperature stress level S v .

[0059] Step 6: Construct a preliminary degradation model.

[0060] In this step, a preliminary degradation model of the aluminum-plated film is constructed to lay the foundation for the subsequent experimental design. Specifically, considering the influence of temperature and humidity stress, the degradation model of the aluminum-plated film is constructed using the Wiener process as follows:

[0061] Y = α0·exp(α1·s T +α2·s RH )·t+σB(t)

[0062] Where Y is the solar absorption ratio or hemispherical emissivity of the aluminum film, t is the degradation time, B() is the standard Brownian motion, σ is the drift coefficient, s T is the normalized temperature stress, s RH is the normalized humidity stress, α0~α2 are model parameters. The unknown parameters of the above degradation model include θ=(α0, α1, α2, σ).

[0063] In the above degradation model, the form of stress normalization depends on its stress type and can be determined by the following formula:

[0064]

[0065] Among them, s is the stress magnitude of the aluminum film during operation, s0 and s H are the normal and maximum applied stress levels, respectively. For temperature stress, the Arrhenius model should be selected. For humidity stress, the power law model should be selected.

[0066] Furthermore, based on the historical data of aluminum-plated films, the maximum likelihood estimation method is used to preliminarily estimate the unknown parameters of the above degradation model. The logarithmic maximum likelihood function lnL of the above degradation model is:

[0067]

[0068] Where k = 4, is the number of stress levels, n l is the number of samples under the lth stress level, m li is the number of performance tests of the i-th sample under the l-th stress level, y lij is the performance value of the i-th sample at the k-th test under the l-th stress level, t lij is the corresponding measurement time, Δy lij =y li(j+1) -y lij is the corresponding degradation increment, Δt lij =t li(j+1) -t lij .

[0069] Step 7: Based on the preliminary degradation model constructed in Step 6 and the actual critical temperature stress level determined in Step 5, design a storage test plan and determine the test stress level.

[0070] Specifically, the D optimization strategy is a commonly used optimization criterion in accelerated storage test design. It maximizes the determinant of the Fisher information matrix to make the parameter estimation obtained from the test data most accurate. The Fisher information matrix can be expressed as:

[0071]

[0072] Each element in the above information matrix is ​​the expectation of the second-order partial derivative of the above logarithmic maximum likelihood function with respect to the unknown parameter.

[0073] Specifically, the goal of the test optimization is to determine the size of the four groups of stress levels of the test, each group includes temperature and humidity stress levels, and the range of stress levels is continuous, which makes it difficult to solve the optimization model. Therefore, in this implementation, the stress application range of the test is discretized, specifically:

[0074] (ii) Actual critical temperature stress level S determined according to step 5 v The test temperature range is (S v -20)℃~S v ℃, humidity levels range from 70% to 90%;

[0075] (ii) The selection interval of temperature stress level is 5°C, and the selection interval of humidity stress level is 5%;

[0076] (III) In order to ensure the accuracy of the law exploration, the temperature and humidity at k stress levels should be the same in pairs.

[0077] Furthermore, based on the above discretization criteria, the experimental scheme optimization model is obtained as follows:

[0078] max det(I)

[0079]

[0080] Where det(I) is the determinant of the Fisher information matrix, is the,th temperature stress level, is the th humidity stress level. Solve the above optimization model and obtain the optimal accelerated storage test plan.

[0081] Step 8: Design stress loading method.

[0082] In this step, in order to avoid condensation when the aluminum-plated film is taken out of the temperature and humidity chamber, which affects the detection of performance parameters, this embodiment adopts the following temperature and humidity stress loading method:

[0083] (i) Maintain at a temperature of 30°C and a humidity of 30% for 30 minutes;

[0084] (ii) Maintaining humidity, use a heating rate of 1°C / min to bring the temperature to the given test stress level;

[0085] (iii) Maintain the temperature and use a humidity increase rate of 1% / min to make the humidity reach the given test stress level;

[0086] (iv) maintaining the temperature and humidity stress for 12 hours;

[0087] (V) Maintain the temperature and use a dehumidification rate of 1% / min to make the humidity reach 30%;

[0088] (vi) Maintain humidity and cool the temperature to 30°C at a rate of 1°C / min.

[0089] According to the above temperature and humidity stress application method, taking the temperature of 65℃ and the humidity of 75% as an example, the test section is shown in Figure 3 .

[0090] Step 9, determine the test equipment and carry out accelerated storage test of aluminum-plated film.

[0091] The test equipment used in the present invention is a temperature and humidity chamber. The number of aluminum-coated film samples under 4 stress levels is 12, and the detection interval of the performance parameters is 12 hours. After the 12 aluminum-coated film samples are clamped by the clamp designed in step 3, they are placed in a temperature and humidity chamber, and the accelerated storage test of the aluminum-coated film is carried out according to the test scheme determined in step 7 and the stress loading method designed in step 8. Before the start of the test, the design scheme of steps 1 and 2 is adopted to test the hemispherical emissivity and solar absorption ratio of each aluminum-coated film sample three times, and the average value is taken as the initial performance value of each sample. Subsequently, every time the detection interval of the performance parameters is reached, all samples are taken out of the temperature and humidity chamber, and the hemispherical emissivity and solar absorption ratio of each sample are tested three times, and the average value is taken and recorded until the test time reaches the deadline.

Claims

1. Accelerated storage test method for aluminum-plated films, characterized in that: The specific steps are as follows: Step 1: Determine the performance parameters of the aluminum film that degrade under storage conditions, including hemispherical emissivity and solar absorptivity; Step 2: Determine the testing equipment, testing steps and testing requirements for the performance parameters of the aluminum-plated film described in step 1; Step 3: Design the fixture for the aluminum film; Step 4: Determine the theoretical critical temperature stress level for the change of the degradation mechanism of the aluminum film as S v ; Step 5: Determine the actual critical temperature stress level at which the degradation mechanism of the aluminum film changes according to the step stress test method; Step 6: Construct a preliminary aluminum film degradation model; Step 7: Based on the preliminary degradation model constructed in step 6 and the actual critical temperature stress level determined in step 5, design a storage test plan and determine the test stress level; In the storage test program design, the stress application range of the test is discretized, and the discretization criterion is: (i) According to the critical temperature stress level determined in step 4, set the temperature level range and humidity level range of the test; (ii) The selection interval of temperature stress level is 5°C, and the selection interval of humidity stress level is 5%; (3) In order to ensure the accuracy of the law exploration, the temperature and humidity at k stress levels should be the same in pairs; Based on the above discretization criteria, the D optimization strategy of maximizing the Fisher information matrix is ​​adopted to obtain the test scheme optimization model; by solving the optimization model, the optimal accelerated storage test scheme is obtained; Step 8: Design stress loading method; Step 9, determine the test equipment and carry out accelerated storage test of aluminum-plated film; After the aluminum-coated film sample is clamped by the fixture designed in step 3, it is placed in a temperature and humidity chamber, and the accelerated storage test of the aluminum-coated film is carried out according to the test plan determined in step 7 and the stress loading method designed in step 8; before the start of the test, the design plan of step 2 is adopted to test the hemispherical emissivity and solar absorption ratio of each aluminum-coated film sample three times, and the average value is taken as the initial performance value of each sample; subsequently, every time the detection interval of the performance parameters is reached, all samples are taken out of the temperature and humidity chamber, and the hemispherical emissivity and solar absorption ratio of each sample are tested three times, and the average value is taken and recorded until the test time reaches the deadline.

2. The accelerated storage test method for aluminum-plated film according to claim 1, characterized in that: The detection equipment in step 2 includes a hemispherical emissivity tester for detecting hemispherical emissivity and a spectrophotometer for detecting solar absorption ratio; wherein the detection steps of the hemispherical emissivity are: (i) Place the probe of the hemispherical emissivity tester on the gold-plated mirror and black material reference samples, and automatically calibrate the instrument according to the reflected energy; (ii) After the calibration is completed, place the aluminum-coated film on the heat sink material table, place the probe of the hemispherical emissivity tester at the center of the aluminum-coated surface of the sample to be tested, and start data testing; (III) Wait for 1 minute for the reading to stabilize, then read and record the value; The above process is carried out three times, and the arithmetic mean of the three measurement results is taken as the hemispherical emissivity of the measured sample; Specifically, the detection steps of solar absorption ratio are as follows: (1) Start the spectrophotometer and connect it to the computer. Preheat the equipment for 1 hour. (ii) Place the standard white plate in the sample chamber and perform self-calibration of the UV-visible spectrophotometer; (iii) After the spectrophotometer self-calibration is completed, remove the standard white plate from the sample chamber; (iv) Place the aluminized film into the sample chamber so that the center of the aluminized surface of the sample to be tested faces the spectrophotometer, and close the sample chamber; (V) Start the test and record the test results after the test is completed.

3. The accelerated storage test method for aluminum-plated film according to claim 1, characterized in that: The detection requirements in step 2 are: the effective measuring surface of the aluminized film shall not be less than 55mm in diameter; the vertical height of the aluminized film shall not be less than 20mm from the ground.

4. The accelerated storage test method for aluminum-plated film according to claim 1, characterized in that: The aluminized film clamp includes an upper clamp and a lower clamp, both of which are made of 0.25mm thick white polyethylene plastic. The two clamps are of the same size and are arranged up and down to clamp the aluminized film between them. When clamping, first use high temperature and high humidity resistant tape to fix one side of the aluminized film on one of the clamps, and then cover the other side of the aluminized film with the other clamp, and bond the two clamps with the tape.

5. The accelerated storage test method for aluminum-plated film according to claim 4, characterized in that: A 70mm*70mm square hole is cut out in the center of the upper and lower clamping surfaces to meet the detection requirement that the effective measuring surface of the aluminum-coated film is not less than 55mm in diameter; at the same time, a clamping surface support part is reserved outside the square hole of the clamping surface. By installing the clamping surface support structure, the detection requirement that the aluminum-coated film is not less than 20mm vertically from the ground is met.

6. The accelerated storage test method for aluminum-plated films according to claim 1, characterized in that: The method for determining the actual critical temperature stress level in step 5 is as follows: according to the theoretical critical temperature stress level of 60°C determined in step 5, a step temperature stress test is carried out starting from 50°C with a stress interval of 2°C, and the actual critical temperature stress level is determined according to the degradation rate of the performance of the aluminum-plated film; a 60-hour storage test is carried out at each temperature stress level, wherein the performance parameters of the aluminum-plated film are determined once every 12 hours using the method in step 2, and a total of 6 performance parameters including the initial performance parameters are collected, and the degradation rate is calculated; if the degradation rate at the current temperature stress level is less than the degradation rate at the previous temperature stress level, the current temperature stress level is the actual critical temperature stress level.

7. The accelerated storage test method for aluminum-plated films according to claim 1, characterized in that: In step 6, the degradation model of the aluminum-plated film is constructed using the Wiener process: Y=α0·exp(α1·s T +α2·s RH )·t+σB(t) Where Y is the solar absorption ratio or hemispherical emissivity of the aluminum film, t is the degradation time, B() is the standard Brownian motion, σ is the drift coefficient, s T is the normalized temperature stress, s RH is the normalized humidity stress, α0~α2 are model parameters; the unknown parameters of the degradation model include θ=(α0, α1, α2, σ); In the above degradation model, the form of stress normalization depends on its stress type and is determined by the following formula: Among them, s is the stress magnitude of the aluminum film during operation, s0 and s H are normal and maximum applied stress levels, respectively; for temperature stress, the Arrhenius model is selected; for humidity stress, the power law model is selected; Furthermore, based on the historical data of aluminum-plated films, the maximum likelihood estimation method is used to preliminarily estimate the unknown parameters of the above degradation model; the logarithmic maximum likelihood function lnL of the above degradation model is: Where k = 4, is the number of stress levels, n l For the l The number of samples at each stress level, m li is the number of performance tests of the i-th sample under the l-th stress level, y lij is the performance value of the i-th sample at the k-th test under the l-th stress level, t lij is the corresponding measurement time, Δy lij =y li(j+1) -y lij is the corresponding degradation increment, Δt lij =t li(j+1) -t lij .

8. The accelerated storage test method for aluminum-plated films according to claim 1, characterized in that: In step 7, the temperature level range of the test is (S v -20)℃~S v ℃; humidity level ranges from 70% to 90%; the obtained test scheme optimization model is: max det(I) Where det(I) is the determinant of the Fisher information matrix, is the lth temperature stress level, is the lth humidity stress level.

9. The accelerated storage test method for aluminum-plated films according to claim 1, characterized in that: In step 8, the temperature and humidity stress loading method is: (i) Maintain at a temperature of 30°C and a humidity of 30% for 30 minutes; (ii) Maintaining humidity, use a heating rate of 1°C / min to bring the temperature to the given test stress level; (iii) Maintain the temperature and use a humidity increase rate of 1% / min to make the humidity reach the given test stress level; (iv) maintaining the temperature and humidity stress for 12 hours; (V) Maintain the temperature and use a dehumidification rate of 1% / min to make the humidity reach 30%; (vi) Maintain humidity and cool the temperature to 30°C at a rate of 1°C / min.

10. The accelerated storage test method for aluminum-plated films according to claim 1, characterized in that: The test equipment used in step 9 is a temperature and humidity chamber.