Method for accurately measuring impurity elements in rhodium powder without interference of rhodium matrix

By establishing a calibration curve of rhodium-containing matrix and rhodium-free matrix in rhodium powder samples, the problem of interference and dissolution of rhodium-based matrix is ​​solved, and the accurate determination of impurities in rhodium powder is achieved, reducing costs and improving detection accuracy.

CN118914166AActive Publication Date: 2024-11-08CHANGCHUN GOLD RES INST
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411300675.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-08
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

In the existing rhodium powder impurity detection methods, rhodium matrix interference leads to inaccurate test results, and conventional standard addition methods are difficult to completely dissolve rhodium powder, which increases experimental costs and errors.

Method used

By weighing an equal amount of rhodium powder sample for microwave digestion and heating concentration, a calibration curve of rhodium-containing substrate and rhodium-free substrate was established. The concentration of impurity elements was detected by inductively coupled plasma atomic emission spectrometer, and the impurity elements in rhodium powder were calculated. content.

Benefits of technology

It effectively eliminates the interference of rhodium matrix on impurity element determination, reduces the testing cost, ensures the accuracy of the results, simplifies the operation process, and is suitable for the determination of impurity element in rhodium powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047562150000041
    Figure BDA0005047562150000041
  • Figure BDA0005047562150000071
    Figure BDA0005047562150000071
  • Figure BDA0005047562150000091
    Figure BDA0005047562150000091
Patent Text Reader

Abstract

The invention provides a method for accurately measuring impurity elements in rhodium powder without interference of a rhodium matrix, and belongs to the field of analysis and detection. The method comprises the following steps: weighing a plurality of equivalent rhodium powder samples, respectively preparing the rhodium powder samples into sample solutions, respectively establishing a calibration curve of a rhodium-containing matrix and a calibration curve of a rhodium-free matrix by adopting an improved standard addition method based on an inductively coupled plasma atomic emission spectrometer, and calculating the calibration curve of the rhodium-containing matrix and the calibration curve of the rhodium-free matrix. The method is used for respectively measuring the content of impurity elements in a to-be-measured sample solution and a to-be-measured blank solution, and then the content of the impurity elements in the rhodium powder can be obtained through calculation. The method not only eliminates interference of rhodium in a matrix on impurity element content determination, but also eliminates system errors caused by deviation of impurity element determination results in a blank solution, effectively ensures the accuracy of the test results, is simple in operation process, saves test time, and is suitable for industrial production. And the problems of poor reproducibility, poor stability and the like of test results are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of analysis and detection, and in particular to a method for accurately determining impurity elements in rhodium powder by removing interference from a rhodium matrix. Background Art

[0002] Rhodium belongs to the platinum group metals and is mainly used as an anti-corrosion material for catalysts and scientific instruments. It is often used as an electroplating layer in the electronics industry and jewelry processing industry. At present, rhodium is mainly used as an automobile exhaust catalyst in the automotive industry. The automobile manufacturing industry is the largest user of rhodium. With the continuous development of fuel cells and the gradual maturity of fuel cell vehicle technology, the amount of rhodium used in the automotive industry has further increased, and its purity will directly affect the performance of the product. Therefore, it is very important to accurately determine the impurity content in rhodium powder and then calculate the purity data of rhodium powder.

[0003] At present, the commonly used methods for detecting impurities in rhodium powder include inductively coupled plasma emission spectroscopy (ICP-AES) and glow discharge mass spectrometry (GD-MS). Jiang Danping et al. published an article entitled "Comparison of Two Different Methods for Determining the Content of Impurity Elements in Rhodium Powder" in "Measurement and Measurement Technology" Volume 40, Issue 6, 2020. The article detailed and compared the two rhodium powder impurity detection methods mentioned above, reflecting the superiority of the ICP-AES detection method. Among them, when the impurity elements in rhodium powder are determined based on ICP-AES, a working curve is formed based on a standard solution without a rhodium matrix, and then the working curve is used to determine the impurity concentration in the rhodium sample solution. However, the rhodium matrix will seriously interfere with the determination of impurity elements, resulting in inaccurate test results. Therefore, it is necessary to eliminate the interference of the rhodium matrix to improve the accuracy of the test results.

[0004] Usually, the interference of the matrix can be eliminated by matching the pure matrix. For example, the patent with the publication number CN110231333A provides a method for determining impurity elements in alumina. The method uses high-purity aluminum to prepare an aluminum matrix standard solution, and then uses the aluminum matrix standard solution and the standard solutions of other impurity elements as a series of standard solutions, and draws a working curve of the series of standard solutions, thereby eliminating the interference of the aluminum matrix. However, if this method is applied to the determination of impurities in rhodium powder, high-purity rhodium needs to be consumed for matching, and high-purity rhodium is rare and expensive, which greatly increases the experimental cost and limits the application of rhodium powder detection methods.

[0005] In addition, the standard addition method can also be used to eliminate matrix interference. However, the conventional standard addition method is to dissolve a sample with a larger sample size, dilute it, and then take an equal amount of solution for testing. This method makes it difficult to detect impurities in the blank solution after dilution, so the blank solution is generally not measured. However, due to the chemical inertness of rhodium, the dissolution of rhodium powder is extremely difficult. In actual application, it is impossible to completely dissolve a sample with a larger sample size, and it is difficult to obtain high-purity rhodium powder for dilution. This conventional standard addition method is not suitable for the detection of rhodium powder. In addition, if there is a certain concentration of impurities in the blank solution, failure to measure it will result in inaccurate test results and systematic errors. Therefore, how to eliminate the systematic error of impurity elements while eliminating rhodium matrix interference is a major problem currently faced when using ICP-AES to determine the content of impurity elements in rhodium powder.

[0006] In view of this, it is necessary to design an improved method for accurately determining impurity elements in rhodium powder by removing the interference of rhodium matrix to solve the above problems. Summary of the invention

[0007] The purpose of the present invention is to provide a method for accurately determining impurity elements in rhodium powder by removing the interference of rhodium matrix. While eliminating the interference of rhodium matrix on the determination of impurity element content, the systematic error caused by impurity elements in blank solution is also eliminated, so as to effectively ensure the accuracy of the test results and make up for the shortcomings of existing detection methods.

[0008] To achieve the above-mentioned object of the invention, the present invention provides a method for accurately determining impurity elements in rhodium powder by removing interference from rhodium matrix, comprising the following steps:

[0009] S1. Weigh several equal amounts of rhodium powder samples, and perform microwave digestion and heating concentration treatment on each of the rhodium powder samples to obtain several sample solutions;

[0010] S2. In the same manner as in step S1, the blank sample is sequentially subjected to the microwave digestion treatment and the heating concentration treatment to obtain a blank solution;

[0011] S3. After at least one portion of the sample solution is fixed to volume, it is used as a sample solution to be tested; different amounts of a mixed standard solution are added to at least three portions of the sample solution, and after fixed volume, it is used as a standard solution containing a rhodium matrix; the mixed standard solution contains impurity elements to be tested;

[0012] S4. using inductively coupled plasma atomic emission spectrometer to detect the sample solution and the standard solution of the rhodium-containing matrix, establishing a calibration curve of the rhodium-containing matrix according to the test result, and calculating the concentration of impurity elements in the sample solution according to the calibration curve of the rhodium-containing matrix;

[0013] S5. Different amounts of the mixed standard solution were added to a volumetric flask, and then hydrochloric acid solution was added, and the volume was adjusted to a standard solution without rhodium matrix; the blank solution was adjusted to volume as a blank solution to be tested;

[0014] S6. The standard solution of the rhodium-free matrix and the blank solution to be tested are detected by inductively coupled plasma atomic emission spectrometry, a calibration curve of the rhodium-free matrix is ​​established according to the test results, and the concentration of impurity elements in the blank solution to be tested is calculated according to the calibration curve of the rhodium-free matrix;

[0015] S7. Calculate the content of impurity elements in the rhodium powder sample according to the concentration of impurity elements in the sample solution to be tested and the concentration of impurity elements in the blank solution to be tested.

[0016] As a further improvement of the present invention, the microwave digestion process comprises the following steps:

[0017] The rhodium powder sample is placed in a microwave digestion tank, hydrochloric acid solution and hydrogen peroxide solution are added into the microwave digestion tank, and the sample is placed in a digestion instrument for heating.

[0018] As a further improvement of the present invention, in step S1, the mass of each rhodium powder sample is 0.0995-0.1005 g; the density of the hydrochloric acid solution added to the microwave digestion tank is 1.19 g / mL, and the amount added is 9-15 mL; the volume fraction of the hydrogen peroxide solution is 30%, and the amount added is 3-5 mL.

[0019] As a further improvement of the present invention, during the microwave digestion treatment, the temperature for heating in the digestion instrument is 240-260° C., and the heating time is 1-2 hours.

[0020] As a further improvement of the present invention, the temperature of the heating concentration treatment is 180-220° C., and the sample solution and the blank solution are both concentrated to 0.8-1.2 mL.

[0021] As a further improvement of the present invention, in step S3, the mixed standard solution contains one or more of the following metal impurities:

[0022] Platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium, tellurium;

[0023] The concentration of each metal impurity in the mixed standard solution is 5-15 μg / mL.

[0024] As a further improvement of the present invention, in step S3, the preparation method of the standard solution of the rhodium-containing matrix includes: adding 0.5 mL, 1 mL, and 2 mL of the mixed standard solution to the three sample solutions respectively, and fixing the volume to obtain the standard solution of the rhodium-containing matrix.

[0025] As a further improvement of the present invention, in step S5, the preparation method of the standard solution of the rhodium-free matrix includes: adding 0 mL, 0.5 mL, 1 mL, and 2 mL of the mixed standard solution to four volumetric flasks, respectively, and then adding hydrochloric acid solution, and the resulting solution is fixed to volume to obtain the standard solution of the rhodium-free matrix.

[0026] As a further improvement of the present invention, in step S5, the density of the hydrochloric acid solution is 1.19 g / mL, and the amount added is 0.8 to 1.2 mL.

[0027] As a further improvement of the present invention, in step S7, the calculation formula for the content of impurity elements in the rhodium powder sample is:

[0028]

[0029] Among them, ω i represents the mass fraction of the impurity element i in the rhodium powder sample, expressed as a percentage; i represents one of platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium and tellurium;

[0030] C i represents the concentration of impurity element i in the sample solution to be tested, in micrograms per milliliter;

[0031] C bi represents the concentration of impurity element i in the blank solution to be tested, in micrograms per milliliter;

[0032] V represents the volume of the sample solution to be tested, in milliliters;

[0033] m represents the mass of the rhodium powder sample, in grams.

[0034] The beneficial effects of the present invention are:

[0035] 1. The accurate determination method of impurity elements in rhodium powder for removing rhodium matrix interference provided by the present invention, by weighing several equal portions of rhodium powder samples, respectively preparing them into sample solutions, then based on inductively coupled plasma atomic emission spectrometer, using standard addition method to respectively establish calibration curves containing rhodium matrix and calibration curves without rhodium matrix, for respectively determining the content of impurity elements in the sample solution to be tested and the blank solution, and then obtaining the accurate content of impurity elements in rhodium powder by calculation. This method not only eliminates the interference of rhodium in the matrix for the determination of impurity element content, but also eliminates the systematic error caused by the deviation of the impurity element determination result in the blank solution, effectively ensuring the accuracy of the test result, and the method operation process is simple, saving test time.

[0036] 2. The present invention can establish a calibration curve of a rhodium-containing matrix by adding different amounts of mixed standard solutions to the sample solution. The calibration curve of the rhodium-containing matrix is ​​used to calculate the impurity content in the solution to be tested, thereby eliminating the interference of rhodium in the matrix with the determination results of other impurity elements. This method not only reduces the test cost, but also ensures the test accuracy. In addition, the calibration curve of the rhodium-containing matrix can realize continuous determination of multiple rhodium powder samples, saving test time.

[0037] 3. The present invention can be applicable to the determination of impurity elements of rhodium powder by improving the conventional standard addition method. Wherein, the present invention can make each sample completely dissolved by directly taking multiple identical and smaller samples (the weighing sample is about 0.1000g), and then subjecting them to microwave digestion treatment respectively, avoiding the problem of difficulty in dissolving rhodium powder when dissolving a larger sample (the weighing sample is about 1g) in the conventional standard addition method, and saving the test cost. On this basis, the present invention adopts the standard addition method to establish the calibration curve of rhodium-free matrix for the first time, and utilizes the calibration curve of the rhodium-free matrix to measure the impurity content in the blank solution, can accurately measure the impurity element content in the blank sample, eliminates the systematic error, thoroughly eliminates the matrix interference, and makes the test result more accurate. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below in conjunction with specific embodiments.

[0039] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0040] The present invention provides a method for accurately determining impurity elements in rhodium powder by removing interference from a rhodium matrix, comprising the following steps:

[0041] S1. Weigh several equal amounts of rhodium powder samples, and perform microwave digestion and heating concentration treatment on each of the rhodium powder samples to obtain several sample solutions;

[0042] S2. In the same manner as in step S1, the blank sample is sequentially subjected to the microwave digestion treatment and the heating concentration treatment to obtain a blank solution;

[0043] S3. After at least one portion of the sample solution is fixed to volume, it is used as a sample solution to be tested; different amounts of a mixed standard solution are added to at least three portions of the sample solution, and after fixed volume, it is used as a standard solution containing a rhodium matrix; the mixed standard solution contains impurity elements to be tested;

[0044] S4. using inductively coupled plasma atomic emission spectrometer to detect the sample solution and the standard solution of the rhodium-containing matrix, establishing a calibration curve of the rhodium-containing matrix according to the test result, and calculating the concentration of impurity elements in the sample solution according to the calibration curve of the rhodium-containing matrix;

[0045] S5. Different amounts of the mixed standard solution were added to a volumetric flask, and then hydrochloric acid solution was added, and the volume was adjusted to a standard solution without rhodium matrix; the blank solution was adjusted to volume as a blank solution to be tested;

[0046] S6. The standard solution of the rhodium-free matrix and the blank solution to be tested are detected by inductively coupled plasma atomic emission spectrometry, a calibration curve of the rhodium-free matrix is ​​established according to the test results, and the concentration of impurity elements in the blank solution to be tested is calculated according to the calibration curve of the rhodium-free matrix;

[0047] S7. Calculate the content of impurity elements in the rhodium powder sample according to the concentration of impurity elements in the sample solution to be tested and the concentration of impurity elements in the blank solution to be tested.

[0048] Through the above-mentioned method, the present invention can simultaneously eliminate the interference of the rhodium matrix on the impurity content in the sample solution to be tested and the blank solution, and accurately measure the content of impurity elements in the rhodium powder in a relatively simple way.

[0049] Preferably, in step S1, the microwave digestion treatment comprises the following steps: placing the rhodium powder sample in a microwave digestion tank, adding 9-15 mL of a hydrochloric acid solution with a density of 1.19 g / mL and 3-5 mL of a hydrogen peroxide solution with a volume fraction of 30% respectively to the microwave digestion tank containing the rhodium powder sample, placing it in a digestion instrument, heating it to 240-260° C. for 1-2 hours. The number of rhodium powder samples is preferably five, and the mass of each rhodium powder sample is equal, all within the range of 0.0995-0.1005 g.

[0050] By adopting the above method, the rhodium powder can be dissolved quickly and completely, which greatly shortens the heating time, reduces the amount of rhodium powder used, and saves the cost of testing.

[0051] In step S1, the temperature of the heating concentration treatment is preferably 180 to 220°C, and the sample solution is concentrated to 0.8 to 1.2 mL.

[0052] The microwave digestion and heating concentration treatment in step S2 are exactly the same as those in step S1, except that no rhodium powder sample is added in step S2 for blank control.

[0053] In step S3, it is preferred to dilute the two sample solutions to use as the sample solutions to be tested so as to improve the accuracy of the test results by averaging; at the same time, it is preferred to add 0.5 mL, 1 mL, and 2 mL of the mixed standard solution to the three sample solutions, respectively, so as to more accurately obtain the calibration curve of the rhodium-containing matrix.

[0054] The mixed standard solution contains one or more of the following metal impurities:

[0055] Platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium, tellurium;

[0056] The concentration of each metal impurity in the mixed standard solution is preferably 5 to 15 μg / mL.

[0057] In step S5, preferably, 0 mL, 0.5 mL, 1 mL, and 2 mL of the mixed standard solution are added to four volumetric flasks, respectively, and then hydrochloric acid solution is added and the volume is fixed. The density of the hydrochloric acid solution is 1.19 g / mL, and the addition amount is preferably 0.8 to 1.2 mL.

[0058] In step S7, the calculation formula for the content of impurity elements in the rhodium powder sample is:

[0059]

[0060] Among them, ω irepresents the mass fraction of the impurity element i in the rhodium powder sample, expressed as a percentage; i represents one of platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium and tellurium;

[0061] C i represents the concentration of impurity element i in the sample solution to be tested, in micrograms per milliliter;

[0062] C bi represents the concentration of impurity element i in the blank solution to be tested, in micrograms per milliliter;

[0063] V represents the volume of the sample solution to be tested, in milliliters;

[0064] m represents the mass of the rhodium powder sample, in grams.

[0065] In the above steps, the volume of the solution after dilution is the same, and preferably a 10 mL volumetric flask is used for dilution.

[0066] The present invention is described in detail below with reference to specific embodiments.

[0067] Example 1

[0068] This embodiment provides a method for accurately determining impurity elements in rhodium powder by removing interference from rhodium matrix, comprising the following steps:

[0069] S1. Weigh five rhodium powder samples, each with a mass of 0.1000g, and place them in five microwave digestion tanks respectively. Add 15mL of hydrochloric acid solution with a density of 1.19g / mL (the purity grade is high-grade pure) and 5mL of hydrogen peroxide solution with a volume concentration of 30% to each microwave digestion tank containing the rhodium powder sample, place them in a high-temperature and high-pressure digestion instrument, heat to 260°C, heat for 1h, and then use water to transfer the digested solutions to five polytetrafluoroethylene beakers respectively, heat at 180°C and concentrate to a volume of 1mL to obtain five sample solutions.

[0070] S2. In the same manner as in step S1, two blank samples are subjected to the microwave digestion treatment and the heating concentration treatment in sequence to obtain two blank solutions each with a volume of 1 mL.

[0071] S3. The five sample solutions prepared in step S1 are transferred to 10mL plastic volumetric flasks respectively, and two of the sample solutions are diluted to scale with water as the sample solutions to be tested, which are respectively denoted as A1 and A2, and the volume is denoted as V; 0.5mL, 1mL, and 2mL of the mixed standard solution are added to the other three sample solutions, and the volume is fixed to scale, as standard solutions containing rhodium matrix, which are respectively denoted as A3, A4, and A5.

[0072] Among them, the mixed standard solution contains metal impurities: platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium, and tellurium; and the concentration of each metal impurity in the mixed standard solution is 10μg / mL.

[0073] S4. A1, A2, A3, A4, and A5 obtained in step S3 are detected by inductively coupled plasma atomic emission spectrometer, and a calibration curve of a rhodium-containing matrix is ​​established according to the detection results. The concentration of impurity elements in A1 and A2 is calculated according to the calibration curve of the rhodium-containing matrix, and the average concentration of the two is recorded as C. i .

[0074] S5., in four 10mL plastic volumetric flasks, 0mL, 0.5mL, 1mL, 2mL mixed standard solution was added respectively, and the mixed standard solution was consistent with that used in step S3; 1mL density was added to each volumetric flask, and the hydrochloric acid solution was consistent with that used in step S1, and then the solution was settled to the scale, as the standard solution without rhodium matrix. After the two blank solutions obtained in step S2 were settled to 10mL, as blank solutions to be measured, they were respectively designated as B1 and B2.

[0075] S6. Using an inductively coupled plasma atomic emission spectrometer, the standard solution of the rhodium-free matrix in step S5 and the blank solutions B1 and B2 to be tested are tested, and a calibration curve of the rhodium-free matrix is ​​established according to the test results, and the concentration of the impurity elements in B1 and B2 is calculated according to the calibration curve of the rhodium-free matrix, and the average value of the two concentrations is recorded as C bi .

[0076] S7. The average value C of the concentration of impurity elements in the sample solutions A1 and A2 obtained in step S4 and step S6 i and the average value C of the concentration of impurity elements in the blank solutions B1 and B2 to be tested bi , calculate the content of metal impurities in the sample to be tested according to the following formula:

[0077]

[0078] Among them, ω i represents the mass fraction of the impurity element i in the rhodium powder sample, expressed as a percentage; i represents one of platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium and tellurium;

[0079] C i represents the concentration of impurity element i in the sample solution to be tested, in micrograms per milliliter;

[0080] C birepresents the concentration of impurity element i in the blank solution to be tested, in micrograms per milliliter;

[0081] V represents the volume of the sample solution to be tested, in milliliters;

[0082] m represents the mass of the rhodium powder sample, in grams.

[0083] The contents of impurity elements in the rhodium powder measured in this embodiment are shown in Table 1.

[0084] Table 1 The content of impurity elements in rhodium powder measured in Example 1

[0085]

[0086] To check the accuracy of the above results, the rhodium powder sample of Example 1 was subjected to a spiked recovery experiment, specifically as follows: 0.1000 g of the rhodium powder sample in Example 1 was weighed, 0.5 mL of the mixed standard solution used in Example 1 was added, and the amount of each metallic impurity added was 5 μg, to obtain a spiked sample, and then the impurity content in the spiked sample was measured according to the steps in Example 1, and the recovery was calculated. The results are shown in Table 2.

[0087] Table 2 Spiked recovery test results of Example 1

[0088]

[0089] From the spike recovery test results in the above table, it can be seen that the spike recovery rate is between 96.0% and 104.0%, indicating that this method is accurate and reliable.

[0090] Example 2

[0091] This embodiment provides a method for accurately determining impurity elements in rhodium powder by removing interference from the rhodium matrix. Compared with Example 1, the difference lies in that the volumes of the hydrochloric acid solution and the hydrogen peroxide solution added in the microwave digestion treatment in step S1 and step S2, the heating temperature and time are changed.

[0092] In this embodiment, the amount of hydrochloric acid solution added in step S1 is 9 mL, the amount of hydrogen peroxide solution added is 3 mL, the heating temperature is 240° C., the heating time is 2 h, and the other raw materials and steps are substantially the same as those in Example 1, which will not be repeated here. The content of impurity elements in the rhodium powder measured in this embodiment is shown in Table 3.

[0093] Table 3 Content of impurity elements in rhodium powder measured in Example 2

[0094]

[0095] In order to verify the accuracy of the above results, the rhodium powder sample used in this embodiment was subjected to a spike recovery experiment, and the experimental method was consistent with the spike recovery experiment in Example 1, which will not be repeated here. The spike recovery experimental results of this embodiment are shown in Table 4.

[0096] Table 4 Spiked recovery test results of Example 2

[0097]

[0098] From the spike recovery test results in the above table, it can be seen that the spike recovery rate is between 96.0% and 104.0%, indicating that this method is accurate and reliable.

[0099] Comparative Example 1

[0100] This comparative example provides a method for accurately determining impurity elements in rhodium powder that removes the interference of rhodium matrix. Compared with Example 1, the difference is that in step S1, two rhodium powder samples are digested, and the operation of steps S3 and S4 is not performed. That is, only a calibration curve without rhodium matrix is ​​established in this comparative example, and the impurity concentration in the sample solution to be tested and the blank solution to be tested is calculated according to the standard curve without rhodium matrix. The other steps in this comparative example are roughly the same as in Example 1, and will not be repeated here. The rhodium powder sample tested in this comparative example is the same as that used in Example 1, and the test results are shown in Table 5.

[0101] Table 5 Content of impurity elements in rhodium powder

[0102] element platinum iridium ruthenium aluminum iron silicon silver content(%) 0.0014 0.0854 0.0924 0.0082 0.0114 0.0085 0.0212 element gold copper nickel cadmium antimony tellurium palladium content(%) 0.0056 Not detected 0.0222 Not detected 0.0072 0.0621 Not detected element lead Zinc magnesium cobalt zirconium content(%) 0.0078 0.0441 0.0112 Not detected Not detected

[0103] It can be seen from the data in Comparative Example 1 that in this comparative example, a calibration curve of a rhodium-free matrix is ​​established only based on the standard solution of the rhodium-free matrix. When the impurity content in the rhodium-containing sample solution to be tested is calculated using the curve, the presence of rhodium causes positive interference in the determination of most impurity elements, and the measured impurity element content is high, which seriously affects the accuracy of the measurement result.

[0104] Comparative Example 2

[0105] This comparative example provides a method for accurately determining impurity elements in rhodium powder without interference from rhodium matrix. Compared with Example 1, the difference is that steps S5, S6, and S7 are omitted, that is, the content of impurity elements in the blank solution is not determined, and the other steps are substantially the same as those in Example 1, which will not be repeated here. The rhodium powder sample tested in this comparative example is the same as that used in Example 1, and the test results are shown in Table 6.

[0106] Table 6 Content of impurity elements in rhodium powder

[0107]

[0108] It can be seen from the data in Example 1 that if the content of impurity elements in the blank solution is not determined, the hydrochloric acid, hydrogen peroxide and iron, silicon, aluminum, magnesium and other elements added in the water during the digestion of the blank solution will be ignored, resulting in a higher content of impurity elements in the measured sample and a systematic error. Therefore, it is very necessary to determine the blank solution.

[0109] Comparative Example 3

[0110] This comparative example provides a method for accurately determining impurity elements in rhodium powder without interference from rhodium matrix. Compared with Example 1, the difference is that the operation of steps S5 and S6 is not performed, but the rhodium-containing matrix established in step S4 is directly used as a calibration curve to determine the content of impurities in the blank solution. The other steps are roughly the same as those in Example 1 and are not repeated here. The rhodium powder sample tested in this comparative example is the same as that used in Example 1, and the test results are shown in Table 7.

[0111] Table 7 Content of impurity elements in rhodium powder

[0112] element platinum iridium ruthenium aluminum iron silicon silver content(%) Not detected 0.0453 0.0784 0.0082 0.0114 0.0066 Not detected element gold copper nickel cadmium antimony tellurium palladium content(%) Not detected Not detected 0.0154 Not detected 0.0321 0.0211 Not detected element lead Zinc magnesium cobalt zirconium content(%) Not detected 0.0343 0.0112 Not detected Not detected

[0113] It can be seen from the data in Comparative Example 1 that if the blank solution is directly measured using a standard solution containing a rhodium matrix, due to the different matrices of the two, there is interference in the determination of most impurity elements, which will affect the determination of the impurity element concentration in the blank solution, thereby causing the content of the impurity elements in the rhodium powder finally measured to deviate greatly from the actual content, affecting the accuracy of the measurement results.

[0114] In summary, the present invention provides a method for accurately determining impurity elements in rhodium powder by removing the interference of rhodium matrix, and the calibration curves of rhodium-containing matrix and rhodium-free matrix are respectively established by adopting improved standard addition method, which are used to respectively determine the content of impurity elements in the test solution and the blank solution, and then the content of impurity elements in rhodium powder is obtained by calculation. This method not only eliminates the interference of rhodium in the matrix on the determination of impurity element content, but also eliminates the systematic error caused by the deviation of the determination result of impurity elements in the blank solution, effectively guarantees the accuracy of the test result, and the method is simple and fast, with high sensitivity and reliable results.

[0115] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for accurately determining impurity elements in rhodium powder without interference from rhodium matrix, characterized in that: The following steps are involved: S1. Weigh several equal amounts of rhodium powder samples, and perform microwave digestion and heating concentration treatment on each of the rhodium powder samples to obtain several sample solutions; S2. In the same manner as in step S1, the blank sample is sequentially subjected to the microwave digestion treatment and the heating concentration treatment to obtain a blank solution; S3. After at least one portion of the sample solution is fixed to volume, it is used as a sample solution to be tested; different amounts of a mixed standard solution are added to at least three portions of the sample solution, and after fixed volume, it is used as a standard solution containing a rhodium matrix; the mixed standard solution contains impurity elements to be tested; S4. using inductively coupled plasma atomic emission spectrometer to detect the sample solution and the standard solution of the rhodium-containing matrix, establishing a calibration curve of the rhodium-containing matrix according to the test result, and calculating the concentration of impurity elements in the sample solution according to the calibration curve of the rhodium-containing matrix; S5. Different amounts of the mixed standard solution were added to a volumetric flask, and then hydrochloric acid solution was added, and the volume was adjusted to a standard solution without rhodium matrix; the blank solution was adjusted to volume as a blank solution to be tested; S6. The standard solution of the rhodium-free matrix and the blank solution to be tested are detected by inductively coupled plasma atomic emission spectrometry, a calibration curve of the rhodium-free matrix is ​​established according to the test results, and the concentration of impurity elements in the blank solution to be tested is calculated according to the calibration curve of the rhodium-free matrix; S7. Calculate the content of impurity elements in the rhodium powder sample according to the concentration of impurity elements in the sample solution to be tested and the concentration of impurity elements in the blank solution to be tested.

2. The method for accurately determining impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 1, characterized in that, The microwave digestion process comprises the following steps: The rhodium powder sample is placed in a microwave digestion tank, hydrochloric acid solution and hydrogen peroxide solution are added into the microwave digestion tank, and the sample is placed in a digestion instrument for heating.

3. The method for accurately determining the impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 2, characterized in that, In step S1, the mass of each rhodium powder sample is 0.0995-0.1005 g; the density of the hydrochloric acid solution added to the microwave digestion tank is 1.19 g / mL, and the added amount is 9-15 mL; the volume fraction of the hydrogen peroxide solution is 30%, and the added amount is 3-5 mL.

4. the method for accurately determining the impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 2, is characterized in that, During the microwave digestion treatment, the temperature for heating in the digestion instrument is 240-260° C., and the heating time is 1-2 hours.

5. the method for accurately determining the impurity elements in the rhodium powder that removes the interference of rhodium matrix according to claim 1, is characterized in that, The temperature of the heating concentration treatment is 180-220° C., and both the sample solution and the blank solution are concentrated to 0.8-1.2 mL.

6. The method for accurately determining impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 1, characterized in that, The mixed standard solution contains one or more of the following metal impurities: Platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium, tellurium; The concentration of each metal impurity in the mixed standard solution is 5-15 μg / mL.

7. The method for accurately determining impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 1, is characterized in that, In step S3, the preparation method of the standard solution of the rhodium-containing matrix includes: adding 0.5 mL, 1 mL, and 2 mL of the mixed standard solution to the three sample solutions respectively, and fixing the volumes to obtain the standard solution of the rhodium-containing matrix.

8. The method for accurately determining impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 1, characterized in that, In step S5, the preparation method of the standard solution of the rhodium-free matrix includes: adding 0 mL, 0.5 mL, 1 mL, and 2 mL of the mixed standard solution to four volumetric flasks respectively, and then adding hydrochloric acid solution, and the resulting solution is fixed to volume to obtain the standard solution of the rhodium-free matrix.

9. the method for accurately determining the impurity elements in the rhodium powder that removes the interference of rhodium matrix according to claim 1, is characterized in that, In step S5, the density of the hydrochloric acid solution is 1.19 g / mL, and the amount added is 0.8 to 1.2 mL.

10. The method for accurately determining impurity elements in the rhodium powder that removes the interference of the rhodium matrix according to claim 1, characterized in that, In step S7, the calculation formula for the content of impurity elements in the rhodium powder sample is: Among them, ω i represents the mass fraction of the impurity element i in the rhodium powder sample, expressed as a percentage; i represents one of platinum, iridium, ruthenium, aluminum, iron, silicon, magnesium, silver, palladium, gold, lead, copper, zinc, nickel, cadmium, cobalt, antimony, zirconium and tellurium; C i represents the concentration of impurity element i in the sample solution to be tested, in micrograms per milliliter; C bi represents the concentration of impurity element i in the blank solution to be tested, in micrograms per milliliter; V represents the volume of the sample solution to be tested, in milliliters; m represents the mass of the rhodium powder sample, in grams.

Citation Information

Patent Citations

  • Method for quickly determining gold, palladium, platinum, rhodium, iridium, silver, nickel, copper and iron in rare and precious metal system

    CN102323250A

  • Method for measuring impurity elements aluminum, phosphor and titanium in nickel concentrate ores

    CN108507858A

  • Quick determining method for twenty impurity elements in ingot casting gold dust

    CN109374599A

  • Method for determining impurity elements in alumina

    CN110231333A

  • Method for detecting impurity elements in bulk drug

    CN111678972A