Test method for locking main cause of battery failure

Through in-situ XRD testing and curve analysis, the main cause of failure of lithium-ion batteries is locked, which solves the problems of low accuracy of results and long test cycles in the existing technology, provides accurate analysis support for the failure mechanism of lithium-ion batteries, and promotes battery performance promote.

CN118914857APending Publication Date: 2024-11-08中汽新能(天津)电池科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981757.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has problems in the failure analysis of lithium-ion batteries with low accuracy, many types of test items, and long test cycles, and it is difficult to accurately lock the essential causes of battery failure.

Method used

In-situ XRD testing method is adopted, by extracting the characteristic peaks of the positive and negative electrodes of the battery, combining the dQ/dV and dV/dQ curves, the main cause of battery failure is locked, avoiding battery anatomy and complex assembly processes, and improving the accuracy and efficiency of the analysis.

Benefits of technology

Accurate locking of lithium-ion battery failure is achieved, in-depth analysis of battery failure mechanisms is provided, and battery performance improvement and technical improvement is supported.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118914857A_ABST
    Figure CN118914857A_ABST
Patent Text Reader

Abstract

The invention discloses a test method for locking the main cause of battery failure, which comprises the following steps of: carrying out charge-discharge test on a failure battery of which the cause of failure is to be analyzed and a non-failure battery of which the batch is the same as that of the failure battery, and drawing a dQ / dV curve and / or a dV / dQ curve of the failure battery and the non-failure battery; performing an in-situ XRD test on the fresh battery in the same system as the failed battery, and extracting a dQ / dV curve and / or positive and negative pole characteristic peaks in the dV / dQ curve of the fresh battery; and analyzing and locking the failure main cause of the failure battery based on the dQ / dV curve and / or dV / dQ curve of the failure battery and the non-failure battery by taking the characteristic peaks of the positive electrode and the negative electrode of the fresh battery as a judgment basis. According to the method, in-situ XRD testing is utilized, on the basis that the battery is not damaged, in-situ XRD data and a dQ / dV curve or a dV / dQ curve are coupled, positive and negative electrode characteristic peaks are extracted, the failure main cause of the battery is locked, and technical support is provided for obtaining the cycle stability and thermal safety factors of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery failure evaluation, and in particular to a testing method for locking the main cause of battery failure. Background Art

[0002] Plug-in hybrid vehicles and pure electric vehicles are becoming more and more popular. The power batteries used, lithium-ion batteries with high-nickel layered oxides and graphite as positive and negative electrode materials respectively, have attracted much attention due to their high energy density and are considered to be one of the most promising batteries in the electric vehicle industry.

[0003] In order to further pursue low cost and long driving mileage, researchers continue to increase the nickel content in the positive electrode material and reduce the Co content. However, as the nickel content continues to increase, a key challenge for the commercialization of lithium-ion batteries using ternary positive electrode materials is poor cycle life and thermal instability. Structural phase change is the main reason for the poor cycle performance of this positive electrode material. There are also many problems with graphite negative electrode materials, such as the deposition of metallic lithium or the growth of lithium dendrites during charging, which will cause internal short circuits and thermal runaway in the battery, the continuous growth of the solid electrolyte layer (SEI) on the surface of the negative electrode, and the irreversible consumption of the electrolyte and the lithium source from the positive electrode, and the gradient difference in lithium ion concentration causes the graphite lattice to change from an ordered sheet structure to a disordered structure. With the continuous insertion / deinsertion of lithium ions, the structural degradation of the positive and negative electrode materials will cause the failure of lithium-ion batteries.

[0004] The progress of electrode materials is inseparable from advanced characterization methods. Accurately diagnosing and quickly finding the main factors that cause lithium-ion battery failure has far-reaching significance for lithium-ion battery performance improvement and technological development. At present, the methods for failure analysis of lithium-ion batteries include impedance method, disassembly analysis method, voltage capacity differential method, etc.

[0005] Among them, the impedance method is to obtain intrinsic reaction kinetics data through polarization curves and electrochemical impedance spectroscopy to infer possible electrochemical reaction paths. This method faces uncertainty in practical applications in the field of lithium-ion batteries, because many different physical and chemical processes or different steps of a complex process often have similar characteristics in the electrochemical impedance spectrum and may overlap with each other, making it difficult to interpret the relevant electrochemical reaction processes.

[0006] Among them, when using the disassembly method for failure analysis, the battery needs to be dissected, the positive and negative electrodes need to be taken out, and then they are made into button batteries respectively for electrochemical analysis and testing. This method has the existence of human factors and external influences such as different time and environment in the process of completing multiple steps, resulting in a high defect rate of the final assembled button batteries and the consistency cannot be guaranteed, which will have a great impact on the test results.

[0007] Among them, the voltage-capacity differential law infers the impact of changes in the crystal structure of electrode materials on battery failure based on the movement of the curve peak. The accuracy of this method needs to be further verified in combination with other testing methods to obtain the results.

[0008] Among them, some laboratories use in-situ XRD for failure analysis, but they need to use specific tooling to assemble half-cells during testing, which can promote the study of electrochemical reaction mechanisms. However, the assembly process of tooling batteries is complicated and easily affected by the test environment. It is not easy to accurately and quantitatively control important reaction kinetic parameters such as the reaction active area. In addition, the presence of bulk diffusion and charge transfer characteristics in the electrode makes it difficult to identify the electrochemical reaction mechanism. On the other hand, tooling batteries are often half-cells, and the research rules of half-cells are not completely applicable to full-cells, because the positive and negative electrodes play a role at the same time during the charging and discharging process, which is essentially different from the corresponding reactions of half-cells. Therefore, the overall dynamic study of the full battery can more accurately characterize the true reaction mechanism of commercial lithium ions.

[0009] Research on the failure mechanism of lithium batteries requires the use of advanced characterization methods to conduct a large amount of basic scientific research and accurately analyze the complex physical and chemical reaction processes inside the battery to find out the fundamental cause of battery failure. This is a technical challenge faced by technical personnel in this field. Summary of the invention

[0010] The purpose of the present invention is to overcome the shortcomings and defects of the prior art and provide a testing method for locking the main cause of battery failure. Based on in-situ XRD testing, the main cause of battery failure can be accurately locked by extracting the characteristic peaks of the positive and negative electrodes of the battery. This method does not require dissection of the battery, solves the problems of low accuracy of failure analysis results, many types of test items, and long test cycles, and provides important data support for in-depth research on the failure mechanism of the battery.

[0011] A method for testing the main cause of battery failure, comprising the steps of:

[0012] Performing charge and discharge tests on the failed battery whose failure cause is to be analyzed and the non-failed batteries in the same batch as the failed battery under the same conditions, and using the obtained charge and discharge data to draw the dQ / dV curve and / or dV / dQ curve of the failed battery and the non-failed battery;

[0013] Performing in-situ XRD testing on a fresh battery of the same system as the failed battery, extracting the dQ / dV curve of the fresh battery and / or the positive and negative characteristic peaks in the dV / dQ curve;

[0014] Taking the extracted dQ / dV curve and / or the positive and negative characteristic peaks in the dV / dQ curve of the fresh battery as the judgment basis, based on the dQ / dV curve and / or dV / dQ curve of the failed battery and the non-failed battery, the main cause of failure of the failed battery is analyzed and the main cause of failure of the failed battery is locked.

[0015] The fresh battery comprises positive and negative electrodes of the same system as the failed battery, and is preferably a soft-pack battery.

[0016] The in-situ XRD test on a fresh battery of the same system as the failed battery comprises:

[0017] The charge and discharge program and the XRD test program are started simultaneously for the fresh battery, and the battery is subjected to in-situ XRD test;

[0018] After the test is completed, the in-situ XRD test results are analyzed, the peak position of each positive and negative electrode characteristic peak determined during the charge and discharge process is read, and the peak position change rate between each positive and negative electrode characteristic peak is quantified;

[0019] The scanning time of each XRD diffraction peak is corresponded to the battery charging and discharging time, and the state of charge SOC of the battery corresponding to each XRD diffraction peak is determined. The SOC range of the electrochemical reaction process dominated by the positive and negative electrodes is determined based on the quantified peak position change rate of the positive and negative electrode characteristic peaks.

[0020] The step of extracting the positive and negative characteristic peaks in the dQ / dV curve and / or the dV / dQ curve of a fresh battery in the same system as the failed battery comprises:

[0021] The battery charge and discharge data can be used to draw the dQ / dV curve and / or dV / dQ curve of a fresh battery. According to the starting SOC and ending SOC corresponding to the SOC interval where the electrochemical reaction process dominated by the positive and negative electrodes of the battery is located, the intervals where the characteristic peaks in the dQ / dV curve and / or dV / dQ curve of the fresh battery are located are divided, and the positive and negative electrode characteristic peaks in the dQ / dV curve and / or dV / dQ curve of the fresh battery are extracted.

[0022] Wherein, the charging and discharging procedure includes:

[0023] Let it stand for T1 time, then charge to the cut-off voltage with the charging current of C1, let it stand for T2 time after the fresh battery is fully charged, then discharge to the cut-off voltage with the discharge current of C2 and let it stand for T3 time; T1, T2, T3 are greater than or equal to the time taken to scan one XRD curve.

[0024] Wherein, the XRD test procedure includes:

[0025] According to the type of positive and negative electrode materials of the battery, set the starting angle, ending angle, step size or scan rate of the XRD test.

[0026] Wherein, the fresh battery is subjected to a charge and discharge procedure and an XRD test procedure after formation, and an in-situ XRD test is performed.

[0027] The analyzing the main cause of failure of the failed battery and identifying the main cause of failure of the failed battery includes:

[0028] The dQ / dV curves and / or dV / dQ curves of the failed battery and the non-failed battery are plotted in the same graph, and then compared and judged based on the positive and negative characteristic peaks extracted from the dQ / dV curves and / or dV / dQ curves of the fresh battery.

[0029] The analyzing the main cause of failure of the failed battery and identifying the main cause of failure of the failed battery includes:

[0030] If the shape and position of the positive electrode characteristic peak in the dQ / dV curve corresponding to the failed battery change significantly compared with the non-failed battery, it proves that the positive electrode failure is the main cause of failure of the failed battery. Conversely, if the shape and position of the negative electrode characteristic peak in the dQ / dV curve corresponding to the failed battery change significantly, it proves that the negative electrode failure is the main cause of failure of the failed battery.

[0031] The analyzing the main cause of failure of the failed battery and identifying the main cause of failure of the failed battery includes:

[0032] If the shape and position of the positive electrode characteristic peak in the dV / dQ curve corresponding to the failed battery change significantly compared with the non-failed battery, it proves that the positive electrode failure is the main cause of failure of the failed battery. Conversely, if the shape and position of the negative electrode characteristic peak in the dV / dQ curve corresponding to the failed battery change significantly, it proves that the negative electrode failure is the main cause of failure of the failed battery.

[0033] The test method for locking the main cause of battery failure of the present invention utilizes in-situ XRD testing. On the basis of not damaging the battery, the in-situ XRD data is coupled with the incremental capacity curve dQ / dV or the voltage capacity differential curve dV / dQ to extract the positive and negative electrode characteristic peaks, thereby providing technical support for obtaining the determining factors of battery cycle stability and thermal safety, which is beneficial to clarifying the improvement direction of lithium-ion batteries and facilitating targeted improvements in the next step.

[0034] The present invention couples the in-situ XRD data with the dQ / dV and / or dV / dQ curves, and can distinguish the characteristic peaks of the electrochemical reactions corresponding to the positive and negative electrodes during the charge and discharge process, so as to identify the main cause of failure of the failed battery and provide technical support for building a failure cause database.

[0035] The present invention can monitor positive and negative electrode materials in real time during the charging and discharging process through the battery in-situ XRD testing technology, and can establish a failure cause database of positive and negative electrode materials of different types of batteries; the in-situ XRD test result is coupled with a dQ / dV curve and / or a dV / dQ curve, so as to realize the extraction of failure characteristic peaks of the positive and negative electrodes of the battery, and to identify the main failure cause of the battery; the in-situ XRD test result is coupled with a dQ / dV curve and / or a dV / dQ curve for failure analysis, which solves the problem that the traditional off-line analysis method cannot obtain the complete dynamic process of the positive and negative electrodes as a whole during the charging and discharging process, and improves the accuracy and efficiency of the battery failure analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Flow chart of a method for testing the main cause of battery failure according to an embodiment of the present invention.

[0037] Figure 2 This is an in-situ XRD data diagram of a fresh battery in an embodiment of the present invention.

[0038] Figure 3 Schematic diagram of the region to which the positive and negative characteristic peaks belong in the dQ / dV curve in an embodiment of the present invention.

[0039] Figure 4 Schematic diagram of the region to which the positive and negative characteristic peaks belong in the dV / dQ curve in an embodiment of the present invention.

[0040] Figure 5 dQ / dV curve comparison diagram of a failed battery and a non-failed battery (normal battery) according to an embodiment of the present invention.

[0041] Figure 6 dV / dQ curve comparison diagram of a failed battery and a non-failed battery (normal battery) according to an embodiment of the present invention.

[0042] Figure 2 and Figure 3 middle:

[0043] Negative-Ⅰ, negative-Ⅱ, negative-Ⅲ, and negative-Ⅳ are the regions to which the negative electrode characteristic peaks belong respectively; positive-Ⅰ, positive-Ⅱ, positive-Ⅲ, and positive-Ⅳ are the regions to which the positive electrode characteristic peaks belong respectively. DETAILED DESCRIPTION

[0044] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0045] The test method for locking the main cause of battery failure in an embodiment of the present invention uses an in-situ X-ray diffractometer in combination with a charging and discharging device to perform an in-situ XRD test on the battery. During the test, X-rays penetrate the battery to obtain the crystal structure evolution information of the positive electrode material and the negative electrode material during the charging and discharging process. The in-situ XRD data is coupled with the dQ / dV curve and / or the dV / dQ curve to extract the characteristic peaks corresponding to the positive and negative electrode reactions during the charging and discharging process, and the main cause of failure of the battery that has undergone failure tests such as cycle testing, storage testing, rate testing, charge retention testing, and high and low temperature discharge testing is locked.

[0046] See also Figure 1 As shown, the method for testing the main cause of the locking battery failure according to the embodiment of the present invention comprises the steps of:

[0047] S1. Perform charge and discharge tests on the failed battery to be analyzed for the cause of failure and the non-failed batteries of the same batch as the failed battery under the same conditions, and use the obtained charge and discharge data to draw the dQ / dV curve and / or dV / dQ curve of the failed battery and the non-failed battery;

[0048] S2. Perform in-situ XRD testing on a fresh battery of the same system as the failed battery, and extract the positive and negative characteristic peaks in the dQ / dV curve and / or dV / dQ curve of the fresh battery;

[0049] S3. Taking the extracted dQ / dV curve and / or the positive and negative characteristic peaks in the dV / dQ curve of the fresh battery as the basis for judgment, based on the dQ / dV curve and / or dV / dQ curve of the failed battery and the non-failed battery, the main cause of failure of the failed battery is analyzed and the main cause of failure of the failed battery is locked.

[0050] In the above step S1, when the failed battery to be analyzed for the cause of failure and the non-failed batteries in the same batch as the failed battery are subjected to charge and discharge tests under the same conditions, the same small current I1 can be used to perform the charge and discharge tests. After the test is completed, the curve drawn according to the charge and discharge test data can be a dQ / dV curve, a dV / dQ curve, or both.

[0051] In the above step S2, in some embodiments, an in-situ XRD test is performed on a fresh battery of the same system as the failed battery, including:

[0052] S21. Start the charge and discharge program and the XRD test program at the same time, and perform an in-situ XRD test on the battery;

[0053] S22. After the test is completed, the in-situ XRD test results are analyzed, firstly the characteristic peaks of the positive and negative electrode materials are determined, and then the peak positions of each positive and negative electrode characteristic peaks during the charge and discharge process are read respectively, and the peak position change rate between each characteristic peak is quantified;

[0054] S23. The scanning time of each XRD diffraction peak corresponds to the battery charge and discharge time, and the SOC of the battery corresponding to each XRD diffraction peak is determined, and the SOC interval of the electrochemical reaction process dominated by the positive and negative electrodes is determined based on the quantified peak position change rate of the positive and negative electrode characteristic peaks;

[0055] In the above step S2, in some embodiments, the extraction of the positive and negative characteristic peaks in the dQ / dV curve and / or the dV / dQ curve of the fresh battery includes:

[0056] The charge and discharge data of the fresh battery are used to draw the dQ / dV curve of the fresh battery. According to the starting SOC and ending SOC corresponding to the SOC interval where the electrochemical reaction process dominated by the positive and negative electrodes of the fresh battery is located, the intervals where the characteristic peaks in the dQ / dV curve of the fresh battery are located are divided respectively, and then the positive and negative characteristic peaks in the dQ / dV curve of the fresh battery are extracted;

[0057] The charge and discharge data of the fresh battery are used to draw the dV / dQ curve of the fresh battery. According to the starting SOC and ending SOC corresponding to the SOC interval where the electrochemical reaction process dominated by the positive and negative electrodes of the fresh battery is located, the intervals where the characteristic peaks in the dV / dQ curve of the fresh battery are located are divided respectively, and then the positive and negative electrode characteristic peaks in the dV / dQ curve of the fresh battery are extracted.

[0058] The charging and discharging procedure for the fresh battery includes:

[0059] Stand for T1 time, charge to the cut-off voltage with the charging current of C1, stand for T2 time after the battery is fully charged, discharge to the cut-off voltage with the discharge current of C2 and stand for T3 time, where T1, T2, and T3 are greater than or equal to the time taken to scan one XRD curve, and C1 and C2 can be adjusted according to the experimental purpose.

[0060] The XRD test procedure for fresh batteries includes the starting angle, ending angle, step length or scanning speed of the test set according to the type of positive and negative electrode materials of the battery and the purpose of the experiment.

[0061] In the above step S3, in some embodiments, the dQ / dV curves of the failed battery and the non-failed battery obtained in step S1 are plotted in the same figure; then, the main cause of failure of the failed battery is analyzed based on the positive and negative electrode characteristic peaks extracted from the dQ / dV curve of the fresh battery; if the shape and position of the positive electrode characteristic peak in the dQ / dV curve corresponding to the failed battery are significantly changed compared with the non-failed battery, it is proved that the positive electrode failure is the main cause of failure of the battery; conversely, if the shape and position of the negative electrode characteristic peak in the dQ / dV curve corresponding to the failed battery are significantly changed, it is proved that the negative electrode failure is the main cause of failure of the battery;

[0062] In the above step S3, in some embodiments, the dV / dQ curves of the failed battery and the non-failed battery obtained in step S1 are plotted in the same figure; then, the main cause of failure of the failed battery is analyzed based on the positive and negative electrode characteristic peaks extracted from the dV / dQ curve of the fresh battery; if the shape and position of the positive electrode characteristic peak in the dV / dQ curve corresponding to the failed battery are significantly changed compared with the non-failed battery, it is proved that the positive electrode failure is the main cause of failure of the battery; conversely, if the shape and position of the negative electrode characteristic peak in the dV / dQ curve corresponding to the failed battery are significantly changed, it is proved that the negative electrode failure is the main cause of failure of the battery.

[0063] The present invention is based on in-situ XRD testing and accurately identifies the main cause of battery failure by extracting the characteristic peaks of the positive and negative electrodes of the battery. This method does not require dissection of the battery, solves the problems of low accuracy of failure analysis results, a large number of test items, and a long test cycle, and provides important data support for in-depth research on the failure mechanism of the battery.

[0064] Example:

[0065] In this embodiment, the failed battery is a battery that has been stored at a high temperature of 60 degrees. After storage, the residual capacity retention rate of the failed battery is 93.39%, and the recovery capacity retention rate is 96.57%; the fresh battery subjected to in-situ XRD test is a soft-pack battery with a thickness of 2 mm; the active main material of the positive electrode sheets of all batteries is NCM, and the active main material of the negative electrode sheets is artificial graphite.

[0066] Step 1: Charge and discharge the failed battery and the non-failed battery

[0067] Step 11), performing a charge and discharge test on the failed battery after high-temperature storage at a current of 0.1C, and drawing a dQ / dV curve of the failed battery using the voltage, capacity, and SOC data;

[0068] Step 12), take another non-failed battery from the same batch as the failed battery, and also perform charge and discharge tests at a current of 0.1C, and use the voltage, capacity, and SOC data to draw the dQ / dV curve of the normal battery;

[0069] Step 13) Using the charge and discharge data, the dV / dQ curves of the failed battery and the normal battery can be drawn.

[0070] Step 2: Extract the positive and negative characteristic peaks of fresh batteries in the same system as the failed battery

[0071] Step 21), using the same system of pole pieces as the failed battery, assemble a thin soft-pack battery with a thickness of 2 mm, and form it with a current of 0.5C, and the battery discharge capacity is 1.54Ah;

[0072] Step 22), after the formation is completed, the fresh battery is placed on the in-situ test sample table, the battery tabs are connected to the charging and discharging equipment, and the battery charging and discharging program is set:

[0073] Let it stand for 30 minutes, charge it with a charging current of 0.1C to a cut-off voltage of 4.3V, let it stand for 30 minutes, then discharge it with a discharge current of 0.1C to a cut-off voltage of 2.8V and let it stand for 30 minutes;

[0074] Step 23), set up the XRD test program:

[0075] The angle range is 5-12°, and the time taken to scan one XRD diffraction peak is 30 min;

[0076] Step 24), simultaneously starting the charge and discharge program and the XRD test program, performing an in-situ XRD test on the battery, and collecting in-situ XRD data of the battery;

[0077] Step 25), after the test is completed, the in-situ XRD data is analyzed:

[0078] The characteristic peak at 6.7° in the first XRD diffraction peak is the characteristic peak of the NCM (003) crystal plane of the positive electrode material, and the characteristic peak at 9.5° is the characteristic peak of the C (002) crystal plane of the negative electrode material. Figure 2 , as lithium ions are embedded / de-embedded in the positive and negative electrode materials during the charge and discharge process, the peak positions of the characteristic peaks of the positive electrode material NCM (003) crystal plane and the characteristic peaks of the negative electrode material C (002) crystal plane will undergo reversible changes, read the peak positions of the characteristic peaks of the positive electrode material NCM (003) crystal plane and the characteristic peaks of the negative electrode material C (002) crystal plane in each XRD diffraction peak, and calculate the peak position change rate between the XRD diffraction peaks;

[0079] Step 26), determine the SOC interval to which the electrochemical reaction process dominated by the positive and negative electrode materials belongs:

[0080] The XRD test time is matched with the battery charge and discharge time, and the SOC of the battery corresponding to each XRD diffraction peak is determined, and then the change rate of the peak position of the characteristic peak of the positive electrode material NCM (003) crystal plane and the characteristic peak of the negative electrode material C (002) crystal plane at different SOCs is obtained. Based on the size of the peak position change rate, the SOC range to which the electrochemical reaction process dominated by the positive and negative electrodes belongs can be determined;

[0081] The characteristic peaks of the positive electrode material NCM (003) crystal plane and the peak position change rate of the negative electrode material C (002) crystal plane of different SOC batteries are quantified. The specific data are shown in Tables 1 and 2.

[0082] Table 1 shows the peak position change rates of the positive and negative characteristic peaks of the fresh battery of the present invention when charged to different SOCs; Table 2 shows the peak position change rates of the positive and negative characteristic peaks of the fresh battery of the present invention when discharged to different SOCs.

[0083] Step 27), extract the positive and negative characteristic peaks in the dQ / dV curve:

[0084] The voltage, capacity, and SOC data of a fresh battery during charge and discharge can be used to draw the dQ / dV curve of the battery. According to the starting SOC and ending SOC corresponding to the SOC interval of the electrochemical reaction process dominated by the positive and negative electrodes of the battery, the area where the characteristic peaks in the dQ / dV curve are located can be divided (see Figure 3 ), and then extract the positive and negative electrode characteristic peaks in the dQ / dV curve (see Table 3), and finally obtain the positive and negative electrode characteristic peaks in the dQ / dV curve of the fresh battery.

[0085] Table 3 shows the positive and negative electrode characteristic peaks extracted from the dQ / dV curve in the method of the present invention.

[0086] Step 28), extract the positive and negative characteristic peaks in the dV / dQ curve:

[0087] Using the same method as step 27), the regions where the positive and negative characteristic peaks in the dV / dQ curve are located are divided (see Figure 4 ), and then extract the positive and negative characteristic peaks in the dV / dQ curve (see Table 4).

[0088] Table 4 shows the positive and negative electrode characteristic peaks extracted from the dV / dQ curve in the method of the present invention.

[0089] Step 3: Conduct comparative analysis to identify the main cause of battery failure

[0090] Step 31), in the same figure, with SOC as the horizontal axis, draw the dQ / dV curves of the failed battery and the non-failed battery obtained in the first step, see Figure 5 ;

[0091] Step 32), using the positive and negative characteristic peaks extracted from the dQ / dV curve of the fresh battery as a basis for judging, analyzing the main cause of failure of the failed battery;

[0092] Step 33), by comparing the dQ / dV curve of the non-failed battery with that of the non-failed battery, it is found that the position and shape of the negative electrode characteristic peak of the failed battery when charged to 9.89% SOC and 17% SOC, and discharged to 12.36% SOC and 8.23% SOC are significantly changed, proving that the negative electrode failure is the main cause of the battery failure after the battery has been stored at high temperature;

[0093] Step 34), using the same method as above, compare the dV / dQ curves of the failed battery and the non-failed battery (see Figure 6 ), it was found that the position and shape of the negative electrode characteristic peaks of the failed battery changed significantly when charged to 9.42% SOC and 16.65% SOC and discharged to 15.53% and 11.61% SOC, proving that the negative electrode failure was the main cause of battery failure after high-temperature storage.

[0094] Table 1

[0095]

[0096]

[0097] Table 2

[0098]

[0099] Table 3

[0100]

[0101] Table 4

[0102]

[0103]

[0104] The basic principles and main features of the present invention and the advantages of the present invention are shown and described above. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention.

[0105] Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is therefore intended that all changes falling within the meaning and range of equivalent elements of the claims are included in the present invention.

[0106] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A test method for locking the main cause of battery failure, characterized in that: Includes steps: Performing charge and discharge tests on the failed battery whose failure cause is to be analyzed and the non-failed batteries in the same batch as the failed battery under the same conditions, and using the obtained charge and discharge data to draw the dQ / dV curve and / or dV / dQ curve of the failed battery and the non-failed battery; Performing in-situ XRD testing on a fresh battery of the same system as the failed battery, extracting the dQ / dV curve of the fresh battery and / or the positive and negative characteristic peaks in the dV / dQ curve; Taking the extracted dQ / dV curve and / or the positive and negative characteristic peaks in the dV / dQ curve of the fresh battery as the judgment basis, based on the dQ / dV curve and / or dV / dQ curve of the failed battery and the non-failed battery, the main cause of failure of the failed battery is analyzed and the main cause of failure of the failed battery is locked.

2. The method for testing the main cause of battery failure according to claim 1, characterized in that: The fresh battery includes positive and negative electrodes of the same system as the failed battery, and is preferably a soft-pack battery.

3. The method for testing the main cause of battery failure according to claim 1, characterized in that: The in-situ XRD test on a fresh battery of the same system as the failed battery comprises: The charge and discharge program and the XRD test program are started simultaneously for the fresh battery to perform in-situ XRD test; After the test is completed, the in-situ XRD test results are analyzed, the peak position of each positive and negative electrode characteristic peak determined during the charge and discharge process is read, and the peak position change rate between each positive and negative electrode characteristic peak is quantified; The scanning time of each XRD diffraction peak corresponds to the battery charging and discharging time, and the state of charge (SOC) of the battery corresponding to each XRD diffraction peak is determined. The SOC range of the electrochemical reaction process dominated by the positive and negative electrodes is determined based on the quantified peak position change rate of the positive and negative electrode characteristic peaks.

4. The method for testing the main cause of battery failure according to claim 3, characterized in that: The extracting of the positive and negative characteristic peaks in the dQ / dV curve and / or the dV / dQ curve of a fresh battery in the same system as the failed battery comprises: The charge and discharge data of a fresh battery are used to draw a dQ / dV curve and / or a dV / dQ curve of the fresh battery. According to the starting SOC and the ending SOC corresponding to the SOC interval where the electrochemical reaction process dominated by the positive and negative electrodes of the battery is located, the intervals where the characteristic peaks in the dQ / dV curve and / or the dV / dQ curve of the fresh battery are located are divided respectively, and the positive and negative characteristic peaks in the dQ / dV curve and / or the dV / dQ curve of the fresh battery are extracted.

5. The method for testing the main cause of battery failure according to claim 3, characterized in that: The charging and discharging procedure includes: Let it stand for T1 time, then charge to the cut-off voltage with the charging current of C1, let it stand for T2 time after the fresh battery is fully charged, then discharge to the cut-off voltage with the discharge current of C2 and let it stand for T3 time; T1, T2, T3 are greater than or equal to the time taken to scan one XRD curve.

6. The method for testing the main cause of battery failure according to claim 3, characterized in that: The XRD testing procedure includes: According to the type of positive and negative electrode materials of the battery, set the starting angle, ending angle, step size or scan rate of the XRD test.

7. The method for testing the main cause of battery failure according to claim 1, characterized in that: The fresh battery is subjected to a charge and discharge procedure and an XRD test procedure after formation, and an in-situ XRD test is performed.

8. The method for testing the main cause of battery failure according to claim 1, characterized in that: The analyzing the main cause of failure of the failed battery and locking the main cause of failure of the failed battery includes: The dQ / dV curves and / or dV / dQ curves of the failed battery and the non-failed battery are plotted in the same graph, and then compared and judged based on the positive and negative characteristic peaks extracted from the dQ / dV curves and / or dV / dQ curves of the fresh battery.

9. The method for testing the main cause of battery failure according to claim 1, characterized in that: The analyzing the main cause of failure of the failed battery and locking the main cause of failure of the failed battery includes: If the shape and position of the positive electrode characteristic peak in the dQ / dV curve corresponding to the failed battery change significantly compared with the non-failed battery, it proves that the positive electrode failure is the main cause of failure of the failed battery. Conversely, if the shape and position of the negative electrode characteristic peak in the dQ / dV curve corresponding to the failed battery change significantly, it proves that the negative electrode failure is the main cause of failure of the failed battery.

10. The method for testing the main cause of battery failure according to claim 1, characterized in that: The analyzing the main cause of failure of the failed battery and locking the main cause of failure of the failed battery includes: If the shape and position of the positive electrode characteristic peak in the dV / dQ curve corresponding to the failed battery change significantly compared with the non-failed battery, it proves that the positive electrode failure is the main cause of failure of the failed battery. Conversely, if the shape and position of the negative electrode characteristic peak in the dV / dQ curve corresponding to the failed battery change significantly, it proves that the negative electrode failure is the main cause of failure of the failed battery.